Please wait a minute...
中国腐蚀与防护学报  2006, Vol. 26 Issue (6): 325-328     
  研究报告 本期目录 | 过刊浏览 |
模拟水中硫离子对不锈钢钝化膜破坏作用的光电化学研究
葛红花;周国定;孙月平
上海电力学院
A photoelectrochemical study on passive films of stainless steel in simulated cooling water with sulfide
;;
上海电力学院
全文: PDF(263 KB)  
摘要: 采用光电化学方法研究了模拟冷却水中硫离子对不锈钢钝化膜的破坏作用.结果表明,不锈钢钝化膜显示n-型光响应,最大吸收峰出现在310nm处。不锈钢钝化膜在电位约-0.35V开始出现光电流,随电位升高,光电流增大。钝化膜禁带宽度Eg随电位的升高而减小,并逐渐向铁氧化物的Eg靠近。模拟冷却水中加入硫离子使不锈钢钝化膜的光电流增大,Eg减小。硫离子的浓度越大,测得的光电流越大,而Eg越小,这可归因于钝化膜膜电阻的降低及钝化膜中氧化铬含量的减少。
关键词 不锈钢模拟冷却水光电化学硫离子    
Abstract:The photoelectrochemical measurement of stainless steel in simulated cooling water shows that, the passive film on the stainless steel exhibits n-type photoresponse, and the peak of absorption happens at 310nm. The passive film on stainless steel starts to generate photocurrent at potential about -0.35V. As the potential rises, the photocurrent increases, and the bandgap energy Eg of the passive film fall. The addition of sulfide in the simulated cooling water can increase the photocurrent, and reduce the Eg values of the passive film on stainless steel. The greater the concentration of the sulfide is, the larger the measured photocurrent and the lower will be the Eg. That is attributable to the fall of the film resistance of the passive film and the decrease of content of chromium oxides in the passive film.
Key wordsstainless steel    simulated cooling water    photoelectrochemical study    sulfide
收稿日期: 2006-02-15     
ZTFLH:  TG174.4  
通讯作者: 葛红花     E-mail: honghge@sohu.com

引用本文:

葛红花; 周国定; 孙月平 . 模拟水中硫离子对不锈钢钝化膜破坏作用的光电化学研究[J]. 中国腐蚀与防护学报, 2006, 26(6): 325-328 .

链接本文:

https://www.jcscp.org/CN/Y2006/V26/I6/325

[1]Stimming U.Photoelectrochemical studies of passive films[J].Elec-trochim.Acta,1986,31(4):415-429
[2]Liu X Y,Zhou G D,Yang M Z.A simple method for monitoring theinhibition of copper corrosion based on photopotential measurements[J].J.Electroanal.Chem.,1993,361:265-267
[3]Cai S M,Jiang D L,Zhang J J,et al.Semiconductive properties andphotoelectrochemistry of iron oxide electrodes-IX.Photoresponsesof sintered Zn-doped oxide electrode[J].Electrochim.Acta,1992,37(3):425-428
[4]Marsh J,Gorse D.A photoelectrochemical and AC impedance studyof anodic titanium oxide films[J].Electrochim.Acta,1998,43(7):659-670
[5]Zhou G D,Shao H,Loo B H.A study of the copper electrode behav-ior in borax buffer solutions containing chloride ions and benzotria-zole-type inhibitors by voltammetry and photocurrent responsemethod[J].J.Electroanal.Chem.,1997,421:129-135
[6]Modestov A D,Zhou G D,Ge H H,et al.A study of copper elec-trode behavior in alkaline solutions containing benzotriazole-typeinhibitors by the photocurrent response method and intensity modu-lated photocurrent spectroscopy[J].J.Electroanal.Chem.,1994,375:293-299
[7]Yang M,Chen L,Cai S.Photoelectrochemical study of pitting oniron in borate buffer solution containing inhibitor[J].Corrosion,1997,53(1):11-15
[8]Ge H H,Zhou G D,Liao Q Q,et al.A study of anti-corrosion be-havior of octadecylamine-treated iron samples[J].Appl.Surf.Sci.,2000,156:39-46
[9]Modestov A D,Zhou G D,Ge H H,et al.A study by voltammetryand the photocurrent response method of copper electrode behaviorin alkaline solutions containing chloride ions[J].J.Electroanal.Chem.,1995,380:63-68
[10]Paola A D,Shukla D,Stimming U.Photoelectrochemical study ofpassive films on stainless steel in neutral solutions[J].Electrochim.Acta,1991,36(2):345-351
[11]Ge H H,Zhou G D,Wu W Q.Passivation model of 316 stainlesssteel in simulated cooling water and the effect of sulfide on the pas-sive film[J].Appl.Surf.Sci.,2003,211(1-4):321-334
[12]Ge H H,Zhou G D,Wu W Q.Passivation model of stainless steelin simulated cooling water[J].J.Chin.Soc.Corros.Prot.,2004,24(2):65-70(葛红花,周国定,吴文权.316不锈钢在模拟冷却水中的钝化模型[J].中国腐蚀与防护学报,2004,24(2):65-70)
[13]Sim es A M P,Ferreira M G S,Rondot B,et al.Study of passivefilms formed on AISI 304 stainless steel by impedance measure-ments and photoelectrochemistry[J].J.Electrochem.Soc.,1990,137(1):82-87
[14]Hakiki N E,Cunha Belo M Da,Sim es A M P,et al.Semiconduct-ing properties of passive films formed on stainless steels-Influenceof the alloying elements[J].J.Electrochem.Soc.,1998,145(11):3821-3829
[15]Sim es A M P,Ferreira M G S,Rondot B,et al.Study of passivefilms formed on AISI 304 stainless steel by impedance measure-ments and photoelectrochemistry[J].J.Electrochem.Soc.,1990,137(1):82-87
[16]Yu J G,Song S Z.Study on localized breakdown of passive films onstainless steels by photoelectrochemical method[J].Corros.Sci.Prot.Technol.,1992,4(4):223-228(虞建国,宋诗哲.光电化学方法研究不锈钢钝化膜的局部破坏[J].腐蚀科学与防护技术,1992,4(4):223-228)
[17]Schmuki P,B hni H,Mansfeld F.A photoelectrochemical investi-gation of passive films formed by alternating voltage passivation[J].J.Electrochem.Soc.,1993,140(7):L119-L123
[18]Yan L C,Zhang J X,Wei Z F,et al.Photoelectrochemical investi-gation of A.V.passive film on 304 stainless steel[J].J.Chin.Soc.Corros.Prot.,2005,25(4):209-212(颜立成,张俊喜,魏增福等.不锈钢载波钝化膜的光电化学研究[J].中国腐蚀与防护学报,2005,25(4):209-212)
[1] 冉斗, 孟惠民, 刘星, 李全德, 巩秀芳, 倪荣, 姜英, 龚显龙, 戴君, 隆彬. pH对14Cr12Ni3WMoV不锈钢在含氯溶液中腐蚀行为的影响[J]. 中国腐蚀与防护学报, 2021, 41(1): 51-59.
[2] 左勇, 曹明鹏, 申淼, 杨新梅. MgCl2-NaCl-KCl熔盐体系中金属Mg对316H不锈钢的缓蚀性能研究[J]. 中国腐蚀与防护学报, 2021, 41(1): 80-86.
[3] 王欣彤, 陈旭, 韩镇泽, 李承媛, 王岐山. 硫酸盐还原菌作用下2205双相不锈钢在3.5%NaCl溶液中应力腐蚀开裂行为研究[J]. 中国腐蚀与防护学报, 2021, 41(1): 43-50.
[4] 张浩, 杜楠, 周文杰, 王帅星, 赵晴. 模拟海水溶液中Fe3+对不锈钢点蚀的影响[J]. 中国腐蚀与防护学报, 2020, 40(6): 517-522.
[5] 马鸣蔚, 赵志浩, 荆思文, 于文峰, 谷义恩, 王旭, 吴明. 17-4 PH不锈钢在含SRB的模拟海水中的应力腐蚀开裂行为研究[J]. 中国腐蚀与防护学报, 2020, 40(6): 523-528.
[6] 赵柏杰, 范益, 李镇镇, 张博威, 程学群. 不同类型接触面对316L不锈钢缝隙腐蚀的影响[J]. 中国腐蚀与防护学报, 2020, 40(4): 332-341.
[7] 胡玉婷, 董鹏飞, 蒋立, 肖葵, 董超芳, 吴俊升, 李晓刚. 海洋大气环境下TC4钛合金与316L不锈钢铆接件腐蚀行为研究[J]. 中国腐蚀与防护学报, 2020, 40(2): 167-174.
[8] 秦越强, 左勇, 申淼. FLiNaK-CrF3/CrF2氧化还原缓冲熔盐体系对316L不锈钢耐蚀性能的影响[J]. 中国腐蚀与防护学报, 2020, 40(2): 182-190.
[9] 何壮,王兴平,刘子涵,盛耀权,米梦芯,陈琳,张岩,李宇春. 316L和HR-2不锈钢在盐酸液膜环境中的钝化与点蚀[J]. 中国腐蚀与防护学报, 2020, 40(1): 17-24.
[10] 武栋才,韩培德. 中温时效处理对SAF2304双相不锈钢耐蚀性的影响[J]. 中国腐蚀与防护学报, 2020, 40(1): 51-56.
[11] 骆鸿,高书君,肖葵,董超芳,李晓刚. 磁控溅射工艺对CrN薄膜及其腐蚀行为的影响[J]. 中国腐蚀与防护学报, 2019, 39(5): 423-430.
[12] 付安庆,赵密锋,李成政,白艳,朱文军,马磊,熊茂县,谢俊峰,雷晓维,吕乃欣. 激光表面熔凝对超级13Cr不锈钢组织与性能的影响研究[J]. 中国腐蚀与防护学报, 2019, 39(5): 446-452.
[13] 孙晓光,韩晓辉,张星爽,张志毅,李刚卿,董超芳. 超低碳奥氏体不锈钢焊接接头耐腐蚀性及环保型化学钝化工艺研究[J]. 中国腐蚀与防护学报, 2019, 39(4): 345-352.
[14] 李雨,关蕾,王冠,张波,柯伟. 机械应力对不锈钢点蚀行为的影响[J]. 中国腐蚀与防护学报, 2019, 39(3): 215-226.
[15] 李兆登,崔振东,侯相钰,高丽丽,王维珍,尹建华. 核级316LN不锈钢焊接接头在高温高压水中的腐蚀性能研究[J]. 中国腐蚀与防护学报, 2019, 39(2): 106-113.