Research Progress on Corrosion Behavior of Metallic Materials in Acetic Acid Environment |
LIU Mingming1,2, YANG Xiaobing3, CHEN Xiaoqi3, WANG Zhengbin2( ), ZHENG Yugui2, HE Chunlin4 |
1.Normal College, Shenyang University, Shenyang 110044, China 2.CAS Key Laboratory of Nuclear Materials and Safety Assessment, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China 3.Nantong Cellulose Fibers Co. Ltd., Nantong 226008, China 4.Liaoning Provincial Key Laboratory of Advanced Materials, Shenyang University, Shenyang 110044, China |
|
|
Abstract Acetic acid is an important raw material and plays an important role in the modern chemical industry. However, acetic acid is highly corrosive, which can easily cause corrosion of metallic components, threatening the service safety of equipment. In order to better understanding and preventing the corrosion induced by acetic acid, this paper summarizes the mechanisms, influencing factors (temperature, acetic acid concentration and impurities) and protection measures for corrosion of metals in acetic acid, on the basis of practical corrosion failure cases. It is expected to provide some guidance for selecting proper materials and taking effective measures to protect components serving in acetic acid environments from corrosion.
|
Received: 08 June 2022
32134.14.1005.4537.2022.186
|
|
1 |
Zhang X. Study and optimization of 3D620 acetic acid distillation column [D]. Xi'an: Xi'an University of Architecture and Technology, 2019
|
|
张鑫. 3D620醋酸精馏塔的研究及优化 [D]. 西安: 西安建筑科技大学, 2019
|
2 |
Liang D D, Wei X S, Wang Y, et al. Electrochemical behaviors and passive film properties of Fe-based bulk metallic glass in Cl--containing acetic acid solutions under high temperature [J]. J. Alloy. Compd., 2018, 766: 964
doi: 10.1016/j.jallcom.2018.07.029
|
3 |
Singh S K, Mukherjee A K. Kinetics of mild steel corrosion in aqueous acetic acid solutions [J]. J. Mater. Sci. Technol., 2010, 26: 264
doi: 10.1016/S1005-0302(10)60044-8
|
4 |
Cheng F T, Shi P, Pang G K H, et al. Microstructural characterization of oxide film formed on NiTi by anodization in acetic acid [J]. J. Alloy. Compd., 2007, 438: 238
doi: 10.1016/j.jallcom.2006.08.020
|
5 |
Xiao M. Supply and demand situation and development prospect of acetic acid at home and abroad [J]. Fine Spec. Chem., 2019, 27(10): 21
|
|
肖铭. 国内外醋酸的供需现状及发展前景 [J]. 精细与专用化学品, 2019, 27(10): 21
|
6 |
Kahyarian A, Schumaker A, Brown B, et al. Acidic corrosion of mild steel in the presence of acetic acid: mechanism and prediction [J]. Electrochim. Acta, 2017, 258: 639
doi: 10.1016/j.electacta.2017.11.109
|
7 |
Nešić S. Key issues related to modelling of internal corrosion of oil and gas pipelines-a review [J]. Corros. Sci., 2007, 49: 4308
doi: 10.1016/j.corsci.2007.06.006
|
8 |
Jiang W H. Analysis on the failure of the tube corrosion of dehydration column reboiler [J]. Press. Vess. Technol., 2012, 29(6): 74
|
|
蒋维宏. PTA装置溶剂脱水塔再沸器换热管腐蚀穿孔失效分析 [J]. 压力容器, 2012, 29(6): 74
|
9 |
Qian G H. Corrosion analysis and countermeasures of acetic acid system equipment in PVA production line [J]. China Chem. Trade, 2017, 9(14): 191
|
|
钱光海. PVA生产线醋酸系统设备的腐蚀分析与对策 [J]. 中国化工贸易, 2017, 9(14): 191
|
10 |
Liu H A, Ye J X. Review of corrosion-resistant metal materials for acetic acid [J]. China Stainless, 2015, (2): 33
|
|
刘焕安, 叶际宣. 醋酸用耐腐蚀金属材料评述 [J]. 不锈, 2015, (2): 33
|
11 |
Hu Q, Guo X, Zhang G, et al. The corrosion behavior of carbon steel in CO2-saturated NaCl crevice solution containing acetic acid [J]. Mater. Corros., 2012, 63: 720
|
12 |
Okafor P C, Brown B, Nesic S. CO2 corrosion of carbon steel in the presence of acetic acid at higher temperatures [J]. J. Appl. Electrochem., 2009, 39: 873
doi: 10.1007/s10800-008-9733-x
|
13 |
George K S, Nešić S. Investigation of carbon dioxide corrosion of mild steel in the presence of acetic acid—Part 1: Basic Mechanisms [J]. Corrosion, 2007, 63: 178
doi: 10.5006/1.3278342
|
14 |
Nord H, Bech-Nielsen G. The anodic dissolution of iron—III. Coverage on iron in the active and passive states in acid carboxylate solutions [J]. Electrochim. Acta, 1971, 16: 849
doi: 10.1016/0013-4686(71)85052-1
|
15 |
Veloz M A, González I. Electrochemical study of carbon steel corrosion in buffered acetic acid solutions with chlorides and H2S [J]. Electrochim. Acta, 2002, 48: 135
doi: 10.1016/S0013-4686(02)00549-2
|
16 |
Amri J, Gulbrandsen E, Nogueira R P. Pit growth and stifling on carbon steel in CO2-containing media in the presence of HAc [J]. Electrochim. Acta, 2009, 54: 7338
doi: 10.1016/j.electacta.2009.07.061
|
17 |
Amri J, Gulbrandsen E, Nogueira R P. Numerical simulation of a single corrosion pit in CO2 and acetic acid environments [J]. Corros. Sci., 2010, 52: 1728
doi: 10.1016/j.corsci.2010.01.010
|
18 |
Amri J, Gulbrandsen E, Nogueira R P. The effect of acetic acid on the pit propagation in CO2 corrosion of carbon steel [J]. Electrochem. Commun., 2008, 10: 200
doi: 10.1016/j.elecom.2007.11.028
|
19 |
Zhao S Z, Xu L N, Dou J J, et al. Influence of acetic acid on top localized corrosion of X70 steel pipeline in CO2 containing wet gas [J]. J. Chin. Soc. Corros. Prot., 2016, 36: 231
|
|
赵书振, 许立宁, 窦娟娟 等. 醋酸对X70管线钢CO2湿气顶部腐蚀行为影响 [J]. 中国腐蚀与防护学报, 2016, 36: 231
|
20 |
Li Y Z, Guo X P, Zhang G A. Synergistic effect of stress and crevice on the corrosion of N80 carbon steel in the CO2-saturated NaCl solution containing acetic acid [J]. Corros. Sci., 2017, 123: 228
doi: 10.1016/j.corsci.2017.05.005
|
21 |
Li Y Z, Xu N, Liu G R, et al. Crevice corrosion of N80 carbon steel in CO2-saturated environment containing acetic acid [J]. Corros. Sci., 2016, 112: 426
doi: 10.1016/j.corsci.2016.08.002
|
22 |
Li Y Z, Xu N, Guo X P, et al. The role of acetic acid or H+ in initiating crevice corrosion of N80 carbon steel in CO2-saturated NaCl solution [J]. Corros. Sci., 2017, 128: 9
doi: 10.1016/j.corsci.2017.08.028
|
23 |
Song G L. Potential and current distributions of one-dimensional galvanic corrosion systems [J]. Corros. Sci., 2010, 52: 455
doi: 10.1016/j.corsci.2009.10.003
|
24 |
Tu H L. Corrosion analysis and countermeasures of acetic acid equipment in polyvinyl alcohol production line [J]. Anhui Sci. Technol., 2019, (7): 45
|
|
涂海浪. 聚乙烯醇生产线醋酸系统设备的腐蚀分析与对策 [J]. 安徽科技, 2019, (7): 45
|
25 |
Yu C Y. Discussion of corrosion resulted from acetic acid and selection of structural material [J]. Process Equip. Piping, 2008, 45(6): 53
|
|
余存烨. 醋酸的腐蚀及其结构材料选用探讨 [J]. 化工设备与管道, 2008, 45(6): 53
|
26 |
Sekine I, Masuko A, Senoo K. Corrosion behavior of AISI 316 stainless steel in formic and acetic acid solutions [J]. Corrosion, 1987, 43: 553
doi: 10.5006/1.3583900
|
27 |
Sekine I, Kawase T, Kobayashi M, et al. The effects of chromium and molybdenum on the corrosion behaviour of ferritic stainless steels in boiling acetic acid solutions [J]. Corros. Sci., 1991, 32: 815
doi: 10.1016/0010-938X(91)90026-L
|
28 |
Sekine I, Hatakeyama S, Nakazawa Y. Corrosion behaviour of Type 430 stainless steel in formic and acetic acids [J]. Corros. Sci., 1987, 27: 275
doi: 10.1016/0010-938X(87)90023-0
|
29 |
Hu R Z, Lin C J, Tan J G, et al. Electrochemical study of the corrosion behavior of coalesced copper and SW-206 stainless steel in the acetic-acid solution [J]. Electrochemistry, 1996, 2: 332
|
|
胡荣宗, 林昌建, 谭建光 等. 磷脱氧铜和不锈钢在醋酸介质中腐蚀行为的电化学研究 [J]. 电化学, 1996, 2: 332
|
30 |
Sun Z M, Wang B, Chen J F. Corrosion behavior of metal materials in acetic acid medium [J]. Corros. Prot., 1998, 19: 55
|
|
孙占梅, 王彪, 陈金富. 金属材料在醋酸中的腐蚀行为研究 [J]. 腐蚀与防护, 1998, 19: 55
|
31 |
Skine I, Momoi K. Corrosion behaviour of SUS 329J1 stainless steel in acetic acid solutions [J]. Key Eng. Mater., 1988, 20-28: 3289
doi: 10.4028/www.scientific.net/KEM.20-28.3289
|
32 |
Perren R A, Suter T A, Uggowitzer P J, et al. Corrosion resistance of super duplex stainless steels in chloride ion containing environments: investigations by means of a new microelectrochemical method: I. Precipitation-free states [J]. Corros. Sci., 2001, 43: 707
doi: 10.1016/S0010-938X(00)00087-1
|
33 |
Cheng X Q, Li X G, Yang L X, et al. Corrosion resistance of 316L stainless steel in acetic acid by EIS and Mott-Schottky [J]. J. Wuhan Univ. Technol.-Mat. Sci. Ed., 2008, 23(4): 574
|
34 |
Cheng S S. Stainless steel corrosion behavior study of PTA plants [D]. Xi'an: Xi'an Shiyou University, 2012
|
|
程姗姗. 化纤PTA装置不锈钢材料腐蚀行为研究 [D]. 西安: 西安石油大学, 2012
|
35 |
Yu C Y. Perception and discussion of pitting on stainless steels equipment in acetic acid [J]. Total Corros. Control, 2010, 24(4): 20
|
|
余存烨. 醋酸装置不锈钢设备点腐蚀原因分析与防护措施 [J]. 全面腐蚀控制, 2010, 24(4): 20
|
36 |
Yu C Y. The analysis of corrosion and using material in acetic acid equipments in chemical industry and chemical fibre production [J]. Total Corros. Control, 2007, 21(3): 21
|
|
余存烨. 化工化纤生产中醋酸设备腐蚀与用材分析 [J]. 全面腐蚀控制, 2007, 21(3): 21
|
37 |
Liu G Q, Zhu Z Y, Ke W. Corrosion behavior of stainless steels and nickel based alloys in acetic acid solution [J]. Corros. Sci. Prot. Technol., 2000, 12: 296
|
|
刘国强, 朱自勇, 柯伟. 不锈钢和镍基合金在含溴醋酸中的腐蚀行为 [J]. 腐蚀科学与防护技术, 2000, 12: 296
|
38 |
Yu C Y. Approach and disussion of materials selection for equipment in high temperature impurity containing acetic acid environment [J]. Corros. Prot., 1999, 20: 37
|
|
余存烨. 高温含杂醋酸环境中设备选材的探讨 [J]. 腐蚀与防护, 1999, 20: 37
|
39 |
Li S R, Zuo Y, Tang Y M, et al. The electroplated Pd-Co alloy film on 316L stainless steel and the corrosion resistance in boiling acetic acid and formic acid mixture with stirring [J]. Appl. Surf. Sci., 2014, 321: 179
doi: 10.1016/j.apsusc.2014.10.013
|
40 |
Turnbull A, Ryan M, Willetts A, et al. Corrosion and electrochemical behaviour of 316L stainless steel in acetic acid solutions [J]. Corros. Sci., 2003, 45: 1051
doi: 10.1016/S0010-938X(02)00149-X
|
41 |
Sun Z M, Zhang J. Corrosion cause of 00Cr20Ni25Mo4.5Cu stainless steel in mixed acetic-formic acid containing chloride ion at elevated temperature [J]. Corros. Prot., 2001, 22: 496
|
|
孙占梅, 张军. 高温含杂质醋酸中00Cr20Ni25Mo 4.5Cu不锈钢腐蚀分析 [J]. 腐蚀与防护, 2001, 22: 496
|
42 |
Singh V B, Singh R N. Corrosion and inhibition studies of copper in aqueous solutions of formic acid and acetic acid [J]. Corros. Sci., 1995, 37: 1399
doi: 10.1016/0010-938X(95)00042-I
|
43 |
Otero E, Pardo A, Utrilla M V, et al. The corrosion behaviour of AISI 304L and 316L stainless steels prepared by powder metallurgy in the presence of organic acids [J]. Corros. Sci., 1997, 39: 453
doi: 10.1016/S0010-938X(97)86097-0
|
44 |
Chief of Japan Titanium Association, translated by Zhou L Z. Titanium Materials and Its Applications [M]. Beijing: Metallurgical Industry Press, 2008: 39
|
|
日本钛协会著, 周连在 译. 钛材料及其应用 [M]. 北京: 冶金工业出版社, 2008: 39
|
45 |
Cheng X Q, Li X G, Du C W, et al. Corrosion behavior of stainless steel and nickel based alloy in acetic acid solution [J]. J. Chin. Soc. Corros. Prot., 2006, 26: 70
|
|
程学群, 李晓刚, 杜翠薇 等. 不锈钢和镍基合金在高温高压醋酸溶液中的腐蚀行为 [J]. 中国腐蚀与防护学报, 2006, 26: 70
|
46 |
Liu G Q, Zhu Z Y, Ke W, et al. Corrosion behavior of 304,254 SMO and Hastelloy C-276 in HAc solution containing Br- ion [J]. J. Chin. Soc. Corros. Prot., 2001, 21: 167
|
|
刘国强, 朱自勇, 柯伟 等. 不锈钢在含有溴离子的醋酸溶液中的腐蚀 [J]. 中国腐蚀与防护学报, 2001, 21: 167
|
47 |
Li M C, Zeng C L, Lin H C, et al. Corrosion behavior of 316 stainless steel in solutions containing F-/Cl- ions [J]. J. Chin. Soc. Corros. Prot., 2002, 22: 162
|
|
李谋成, 曾潮流, 林海潮 等. 316不锈钢在F-/Cl-酸性溶液中的腐蚀行为 [J]. 中国腐蚀与防护学报, 2002, 22: 162
|
48 |
Yu C Y. Pit corrosion of stainless steel in PTA unit [J]. Corros. Prot. Petrochem. Ind., 2009, 26(6): 1
|
|
余存烨. PTA装置不锈钢点腐蚀综述 [J]. 石油化工腐蚀与防护, 2009, 26(6): 1
|
49 |
Chaves R, Costa I, Melo H G D, et al. Evaluation of selective corrosion in UNS S31803 duplex stainless steel with electrochemical impedance spectroscopy [J]. Electrochim. Acta, 2006, 51: 1842
doi: 10.1016/j.electacta.2005.02.105
|
50 |
Merello R, Botana F J, Botella J, et al. Determination of the weaker phase in the pitting corrosion of non-standard low-Ni high-Mn-N duplex stainless steels [J]. Mater. Corros., 2004, 55: 95
doi: 10.1002/maco.200303694
|
51 |
Gao X D, Li J K, Ren X P, et al. Effect of solid solution temperature on microstructure and microhardness of 2205 duplex stainless steel [J]. Heat Treat. Met., 2021, 46(1): 7
|
|
高晓丹, 李晶琨, 任学平 等. 固溶温度对2205双相不锈钢组织和硬度的影响 [J]. 金属热处理, 2021, 46(1): 7
|
52 |
Xu Z Q. Study on corrosion mechanism and corrosion protection countermeasures for acetic acid rectifying tower in polyvinyl alcohol plant [J]. Petro-Chem. Equip. Technol., 2008, 29(5): 46
|
|
许志强. PVA车间醋酸塔腐蚀机理研究及防护对策 [J]. 石油化工设备技术, 2008, 29(5): 46
|
53 |
Wang Z B, Hu H X, Zheng Y G, et al. Comparison of the corrosion behavior of pure titanium and its alloys in fluoride-containing sulfuric acid [J]. Corros. Sci., 2016, 103: 50
doi: 10.1016/j.corsci.2015.11.003
|
54 |
Jiang W. Influnce of technological parameter on corrosion for 2205DSS and TA2 in brine and establishment of mathematical model [D]. Zigong: Sichuan University of Science & Engineering, 2008
|
|
蒋伟. 工艺参数对2205DSS与TA2在卤水中的腐蚀影响及其数学模型的建立 [D]. 自贡: 四川理工学院, 2008
|
55 |
Yu C Y. Discussion of crevice corrosion occurred in chemical titanium equipment [J]. Process Equip. Piping, 2010, 47(5): 61
|
|
余存烨. 钛制化工设备缝隙腐蚀探讨 [J]. 化工设备与管道, 2010, 47(5): 61
|
56 |
Zhang Q, Tang R, Yin K J, et al. Corrosion behavior of Hastelloy C-276 in supercritical water [J]. Corros. Sci., 2009, 51: 2092
doi: 10.1016/j.corsci.2009.05.041
|
57 |
Al-Malahy K S E, Hodgkiess T. Comparative studies of the seawater corrosion behaviour of a range of materials [J]. Desalination, 2003, 158: 35
doi: 10.1016/S0011-9164(03)00430-2
|
58 |
Singh V B, Gupta A. The electrochemical corrosion and passivation behaviour of Monel (400) in concentrated acids and their mixtures [J]. J. Mater. Sci., 2001, 36: 1433
doi: 10.1023/A:1017584326909
|
59 |
Lu Y L, Liu J X, Li X K, et al. Hot deformation behavior of Hastelly C276 superalloy [J]. Trans. Nonferrous Met. Soc. China, 2012, 22, suppl.1: s84
|
60 |
Ma G Y, Wu D J, Guo D M. Segregation Characteristics of pulsed laser butt welding of Hastelloy C-276 [J]. Metall. Mater. Trans., 2011, 42A: 3853
|
61 |
Jiao S Y, Zhu G N, Dong J X, et al. Garbide evolution and Mo depletion law in hastelloy C-276 [J]. J. Mater. Eng., 2011, 39(1): 47
|
|
焦少阳, 朱冠妮, 董建新 等. Hastelloy C-276中碳化物析出及晶界贫Mo规律研究 [J]. 材料工程, 2011, 39(1): 47
|
62 |
Wu D J, Fan C, Liu S B, et al. Corrosion performance of laser welding on dissimilar materials hastelloy C-276/316L [J]. Chin. J. Nonferrous Met., 2014, 24: 441
doi: 10.1016/S1003-6326(14)63080-6
|
|
吴东江, 范聪, 刘士博 等. Hastelloy C-276/316L激光异质焊焊缝腐蚀性能 [J]. 中国有色金属学报, 2014, 24: 441
|
63 |
Zheng G H. Corrosion in the production of polyvinyl alcohol and protection technologies [J]. Petrochem. Corros. Prot., 2002, 19(3): 6
|
|
郑国汉. 聚乙烯醇生产过程中的腐蚀与防护技术 [J]. 石油化工腐蚀与防护, 2002, 19(3): 6
|
64 |
Li W. Discussion on corrosion status and anti-corrosion of PTA plant in petrochemical industry [J]. China Plant Eng., 2009, (9): 32
|
|
李旺. 石化PTA装置腐蚀现状与防腐探讨 [J]. 中国设备工程, 2009, (9): 32
|
65 |
Zhang Y M, Li X D, Li M S, et al. Investigation on corrosion of Yizheng chemical fiber [J]. Corros. Sci. Prot. Technol., 2000, 12: 364
|
|
张亚明, 李晓东, 李美栓 等. 仪征化纤化工厂腐蚀情况调查 [J]. 腐蚀科学与防护技术, 2000, 12: 364
|
66 |
Wu X B, Yu Z G. Characteristics and protection of local corrosion on PTA reactors [J]. CFHI Technol., 2013, (3): 22
|
|
吴学彬, 于志刚. PTA反应器的局部腐蚀特点及防护方法 [J]. 一重技术, 2013, (3): 22
|
67 |
Yu C Y, Lin H H. Material selection and corrosion analysis of acetic acid equipment in Shanghai Petrochemical Plant [J]. Petrochem. Technol. Jinshan, 1985, (2): 70
|
|
余存烨, 林宏华. 上海石化总厂醋酸设备选材及腐蚀分析 [J]. 金山石油化工化纤技术, 1985, (2): 70
|
68 |
Miao Y Y, Sun Y E. Corrosion analysis and anticorrosion discussion of PTA plant [J]. Chem. Enterp. Manage., 2016, (5): 193
|
|
苗媛媛, 孙亚娥. PTA装置腐蚀分析及对策探讨 [J]. 化工管理, 2016, (5): 193
|
69 |
Gao X, Tang J L, Zuo Y, et al. The electroplated palladium-copper alloy film on 316L stainless steel and its corrosion resistance in mixture of acetic and formic acids [J]. Corros. Sci., 2009, 51: 1822
doi: 10.1016/j.corsci.2009.05.008
|
No Suggested Reading articles found! |
|
|
Viewed |
|
|
|
Full text
|
|
|
|
|
Abstract
|
|
|
|
|
Cited |
|
|
|
|
|
Shared |
|
|
|
|
|
Discussed |
|
|
|
|