纯Cu和铜包钢在大港土壤环境中的腐蚀行为研究
朱 敏 杜翠薇 李晓刚 刘智勇 王胜荣 李建宽 贾静焕
北京科技大学材料科学与工程学院 北京 100083
Corrosion Behavior of Pure Copper and Copper-clad Steels in Soil at Dagang District
ZHU Min, DU Cuiwei, LI Xiaogang, LIU Zhiyong, WANG Shengrong, LI Jiankuan, JIA Jinghuan
School of Materials Science and Engineering, University of Science and Technology Beijing,Beijing 100083, China
全文: PDF(3837 KB)  
摘要: 通过1 a现场实验,并结合腐蚀形貌宏观观察、SEM、XRD及失重法对纯Cu和铜包钢在大港土壤环境中的腐蚀行为进行了研究。结果表明, 现场埋样的纯Cu、电镀铜包钢和连铸铜包钢的平均腐蚀速率分别为1.01,1.05和1.07 g/(dm2a),其中电镀铜包钢和连铸铜包钢的平均腐蚀速率接近,纯Cu的腐蚀速率略小;腐蚀特征均表现为非均匀的全面腐蚀,腐蚀程度有所差异;腐蚀产物均主要由Cu2O,Cu(OH)2和CuCl组成。
关键词 纯Cu铜包钢大港土壤腐蚀行为    
Abstract:The corrosion behavior of pure copper and copper-clad steels in soil at Dagang district was investigated by burying test in nature field for one year with weight-loss measurement, as well as macro-morphology observation, characterization of corrosion products by SEM and XRD. The results showed that the corrosion rates for pure copper, electroplating copper-clad steel and continuous casting copper-clad steels are 1.01, 1.05 and 1.07 g/(dm2a), respectively. The average corrosion rates of electroplating copper-clad steel and continuous casting copper-clad steel are roughly equal, and that of pure copper is slightly lower than copper-clad steels. Inhomogeneous general corrosion occurs mainly on the pure copper and copper-clad steels in soil at Dagang district, with the different corrosion degree. The corrosion products of pure copper and copper-clad steels consist of Cu2O, Cu(OH)2, CuCl.
Key wordspure copper    copper-clad steel    soil of Dagang    corrosion behavior
收稿日期: 2013-04-02     
ZTFLH:  TG172.4  
基金资助:国家自然科学基金重点项目(51131001) 和 国家自然科学基金项目 (50971016) 资助
通讯作者: 杜翠薇,E-mail:dcw@ustb.edu.cn   
作者简介: 朱敏,男,1985年生,博士生,研究方向为材料的腐蚀与防护

引用本文:

朱敏, 杜翠薇, 李晓刚, 刘智勇, 王胜荣, 李建宽, 贾静焕. 纯Cu和铜包钢在大港土壤环境中的腐蚀行为研究[J]. 中国腐蚀与防护学报, 2013, 33(6): 496-500.
ZHU Min, DU Cuiwei, LI Xiaogang, LIU Zhiyong, WANG Shengrong, LI Jiankuan, JIA Jinghuan. Corrosion Behavior of Pure Copper and Copper-clad Steels in Soil at Dagang District. Journal of Chinese Society for Corrosion and protection, 2013, 33(6): 496-500.

链接本文:

https://www.jcscp.org/CN/      或      https://www.jcscp.org/CN/Y2013/V33/I6/496

[1] Zhou P P, Wang S, Li Z Z, et al. Review of corrosion resistant metals for grounding [J]. Elec. Power Constr., 2010, 31(8): 51-54
(周佩朋, 王森, 李志忠等. 耐蚀性金属接地材料研究综述 [J]. 电力建设, 2010, 31(8): 51-54)
[2] Li J L. Utility Electrical Grounding Technology [M]. Beijing: China Electric Power Press, 2002
(李景禄. 实用电力接地技术 [M]. 北京: 中国电力出版社, 2002)
[3] Yang D W, Li J L. Analysis on corrosion and anti-corrosion measure of substation grounding device [J]. Insul. Surg. Arresters, 2004, (2): 43-46
(杨道武, 李景禄. 发电厂变电所接地装置的腐蚀及防腐蚀措施 [J]. 电瓷避雷器, 2004, (2): 43-46)
[4] Weng Y F. Analysis of grounding connection cauterization and the suggestions for material selection [J]. Zhejiang Elec. Power, 2003, (4): 54-56
(翁羽丰. 接地装置腐蚀分析及材料选用建议 [J]. 浙江电力, 2003, (4): 54-56)
[5] Li Y Q. Analysis of corrosion behavior of common grounding electrode materials [D]. Beijing: University of Science and Technology Beijing, 2010
(李月强. 常用接地电极材料的腐蚀行为研究 [D]. 北京: 北京科技大学, 2010)
[6] Fourez M, Cheno F. The application of Zinc aluminium flake non-electrolytic surface coating [J]. Trans. Inst. Met. Finish., 1993, 71(1): 21-25
[7] Lindsey T. National electrical grounding research project technical report [R]. Massachusetts: The Fire Protection Research Foundation, 2007
[8] Loboda M, Marciniak R. Field corrosion tests in Poland of copper coated steel earthing rods for LPS [A]. 29th International Conference On Lightning Protection [C]. Uppsala, 2008
[9] BS 7430: 1998, Code of practice for earthing [S]
[10] UL467, Standard for grounding and bonding equipment [S]
[11] Wang Q J, Du Z Z, Wang H B. Characteristics and technical status-quo of the manufacturing process for copper-clad steel wire [J]. Elec. Wire Cable, 2002, (4): 15-27
(王庆娟, 杜忠泽, 王海波. 铜包钢线生产工艺的特点及现状 [J].电线电缆, 2002, (4): 15-27)
[12] GB/T 16545-1996, Removal of corrosion products from corrosion test specimens of metals and alloys [S]. Beijing: National Quality Supervision, 1996
(GB/T 16545-1996, 金属和合金的腐蚀试样上腐蚀产物的清除 [S]. 北京: 国家技术监督局, 1996)
[13] Li X G, Du C W, Dong C F, et al. Corrosion Behavior and Test of X70 Pipeline Steel [M]. Beijing: Science Press, 2006
(李晓刚, 杜翠薇, 董超芳等. X70钢的腐蚀行为与试验研究 [M]. 北京: 科学出版社, 2006)
[14] Fitzgerald K P, Nairn J, Skennerton G, et al. Atmospheric corrosion of copper and the colour, structure and composition of natural patinas on copper [J]. Corros. Sci., 2006, 48(9): 2480-2509
[15] Mayer S T, Muller R. An in situ Raman spectroscopy study of the anodic oxidation of copper in alkaline media [J]. J. Electrochem. Soc., 1992, 139: 426-434
[16] Yu B, Woo P, Erb U. Corrosion behaviour of nanocrystalline copper foil in sodium hydroxide solution [J]. Scr. Mater., 2007, 56: 353-356
[17] Kunze J, Maurice V, Klein L H, et al. In situ STM study of the duplex passive films formed on Cu(111) and Cu(001) in 0.1 M NaOH[J]. Corros. Sci., 2004, 46: 245-264
[18] Rosalbino F, Carlini R, Soggia F, et al. In?uence of rare earth metals addition on the corrosion behaviour of copper in alkaline environment [J]. Corros. Sci., 2012, 58: 139-144
[1] 李琳, 陈义庆, 高鹏, 艾芳芳, 钟彬, 伞宏宇, 杨颖. 除冰盐环境下桥梁钢的耐腐蚀性能研究[J]. 中国腐蚀与防护学报, 2020, 40(5): 448-454.
[2] 张欣, 杨光恒, 王泽华, 曹静, 邵佳, 周泽华. 冷拉拔变形过程中含稀土铝镁合金腐蚀行为研究[J]. 中国腐蚀与防护学报, 2020, 40(5): 432-438.
[3] 胡露露, 赵旭阳, 刘盼, 吴芳芳, 张鉴清, 冷文华, 曹发和. 交流电场与液膜厚度对A6082-T6铝合金腐蚀行为的影响[J]. 中国腐蚀与防护学报, 2020, 40(4): 342-350.
[4] 王新华, 杨永, 陈迎春, 位凯玲. 交流电流对X100管线钢在库尔勒土壤模拟液中腐蚀行为的影响[J]. 中国腐蚀与防护学报, 2020, 40(3): 259-265.
[5] 胡玉婷, 董鹏飞, 蒋立, 肖葵, 董超芳, 吴俊升, 李晓刚. 海洋大气环境下TC4钛合金与316L不锈钢铆接件腐蚀行为研究[J]. 中国腐蚀与防护学报, 2020, 40(2): 167-174.
[6] 张尧, 郭晨, 刘妍慧, 郝美娟, 成世明, 程伟丽. 挤压态Mg-2Sn-1Al-1Zn合金在模拟体液中的电化学腐蚀行为[J]. 中国腐蚀与防护学报, 2020, 40(2): 146-150.
[7] 苏小红,胡会娥,孔小东. W颗粒/Zr41.2Ti13.8Cu12.5Ni10Be22.5基非晶复合材料在3%NaCl溶液中的腐蚀行为研究[J]. 中国腐蚀与防护学报, 2020, 40(1): 70-74.
[8] 王勤英,裴芮,西宇辰. 镍基激光熔覆层冲刷腐蚀行为研究[J]. 中国腐蚀与防护学报, 2019, 39(5): 458-462.
[9] 郭铁明,张延文,秦俊山,宋志涛,董建军,杨新龙,南雪丽. 桥梁钢Q345q在3种模拟大气环境中的腐蚀行为研究[J]. 中国腐蚀与防护学报, 2019, 39(4): 319-330.
[10] 黄博博,刘平,刘新宽,梅品修,陈小红. 新型HSn70-1铜网衣两年期海水腐蚀行为研究[J]. 中国腐蚀与防护学报, 2018, 38(6): 594-600.
[11] 曹海娇, 魏英华, 赵洪涛, 吕晨曦, 毛耀宗, 李京. Q345钢预热时间对熔结环氧粉末涂层防护性能的影响II:涂层体系失效行为分析[J]. 中国腐蚀与防护学报, 2018, 38(3): 255-264.
[12] 张杰, 胡秀华, 郑传波, 段继周, 侯保荣. 海洋微藻环境中钙质层对Q235碳钢腐蚀行为的影响[J]. 中国腐蚀与防护学报, 2018, 38(1): 18-25.
[13] 张子阳,王善林,章恒瑜,柯黎明. AZ31镁合金搅拌摩擦焊接头腐蚀行为[J]. 中国腐蚀与防护学报, 2017, 37(2): 117-125.
[14] 刘栓,周开河,方云辉,徐孝忠,江炯,郭小平,郑文茹,蒲吉斌,王立平. 环境因素对纯Zn在饱和Zn(OH)2溶液中腐蚀行为的影响I—Cl-浓度和pH值[J]. 中国腐蚀与防护学报, 2016, 36(6): 522-528.
[15] 周开河,方云辉,徐孝忠,江炯,郭小平,刘栓,郑文茹,蒲吉斌,王立平. 环境因素对纯Zn在饱和Zn(OH)2溶液中腐蚀行为的影响II—温度和溶解氧浓度[J]. 中国腐蚀与防护学报, 2016, 36(6): 529-534.