Please wait a minute...
中国腐蚀与防护学报  2026, Vol. 46 Issue (3): 703-716     CSTR: 32134.14.1005.4537.2025.225      DOI: 10.11902/1005.4537.2025.225
  研究报告 本期目录 | 过刊浏览 |
腐蚀产物对锌合金镀层切边腐蚀行为的影响
李永坤, 周佳顺, 王友彬(), 高锋, 王欣鹏, 汤宏群
广西大学资源环境与材料学院 南宁 530004
Influence of Corrosion Products on Corrosion Behavior of Cut Edges of Galvanized Coatings/Q235 Carbon Steel
LI Yongkun, ZHOU Jiashun, WANG Youbin(), GAO Feng, WANG Xinpeng, TANG Hongqun
School of Resources, Environment and Materials, Guangxi University, Nanning 530004, China
引用本文:

李永坤, 周佳顺, 王友彬, 高锋, 王欣鹏, 汤宏群. 腐蚀产物对锌合金镀层切边腐蚀行为的影响[J]. 中国腐蚀与防护学报, 2026, 46(3): 703-716.
Yongkun LI, Jiashun ZHOU, Youbin WANG, Feng GAO, Xinpeng WANG, Hongqun TANG. Influence of Corrosion Products on Corrosion Behavior of Cut Edges of Galvanized Coatings/Q235 Carbon Steel[J]. Journal of Chinese Society for Corrosion and protection, 2026, 46(3): 703-716.

全文: PDF(28053 KB)   HTML
摘要: 

基于腐蚀产物的防护性能探究锌基共晶合金镀层切边腐蚀行为。选取纯Zn,以及Zn-3Mg、Zn-5Al和Zn-4Al-3Mg 3种锌基共晶合金镀层作为研究对象,通过浸泡实验和盐雾试验的方法,采用扫描电镜(SEM)、能谱仪(EDS)、X射线衍射技术(XRD)等技术分析切边处腐蚀产物物相组成及形貌,采用扫描电化学显微镜(SECM)表征了不同共晶合金镀层切边的微区腐蚀行为。SEM和EDS结果表明,腐蚀产物在切边处的镀层和靠近镀层的钢基体上均有分布,Zn和Zn-3Mg镀层上的腐蚀产物主要为碱式氯化锌(Zn5(OH)8Cl2),钢基体上的腐蚀产物主要为Zn5(OH)8Cl2和碱式碳酸锌(Zn5(OH)6(CO3)2·H2O);Zn-5Al和Zn-4Al-3Mg镀层其腐蚀产物还存在锌铝层状双金属氢氧化物(Zn6Al2(OH)16CO3·4H2O)。SECM表明实验初期Zn-Al镀层与Zn-Al-Mg镀层的反馈电流相较于Zn镀层高,一段时间后Zn-Al镀层与Zn-Al-Mg镀层的反馈电流低于Zn镀层,在镀层表面和远离镀层一侧的钢基体表面的反馈电流较大,靠近镀层一侧的钢基体表面反馈电流较小,且整体反馈电流和电流凹陷随腐蚀时间而降低。盐雾腐蚀实验显示纯Zn镀层、Zn-Mg镀层、Zn-Al镀层与Zn-Al-Mg镀层切边样品的平均失重速率分别为1.04 × 10-2、9.88 × 10-3、5.73 × 10-3和5.21 × 10-3 g·m-1·h-1。Zn-4Al-3Mg镀层的切边耐腐蚀性最好,其腐蚀产物层结构致密,保护性产物Zn5(OH)8Cl2和Zn6Al2(OH)16CO3·4H2O的含量较高,起到了协同防护作用,腐蚀产物层良好的防护性能使得Zn-Al-Mg镀层表现出较优的长久耐蚀性能。

关键词 : 锌基共晶合金,  腐蚀产物,  切边腐蚀,  微区腐蚀,  微区电化学,  腐蚀行为    
Abstract:

Zn-based eutectic alloy coatings with high corrosion resistance and sacrificial anode protection performance are widely used for corrosion protection of steel. During the usage process, galvanized steel plates are often subjected to cutting or shaping operations, which can cause the galvanized coating and/or the steel substrate at the cutting edge to be exposed to environmental corrosion. Then, how the steel substrate at the cutting edge is corroded, and how the adjacent galvanized layer or its corrosion products will affect the corrosion behavior of the steel substrate, are all topics worthy of study. Herein, the corrosion behavior of cut edge of galvanized coatings of pure Zn, Zn-3Mg, Zn-5Al, and Zn-4Al-3Mg/Q235 carbon steel was studied. First the galvanized steels were cut into cylindrical samples, and sealed using epoxy resin, leaving only one cut-edge surface free and polished. The samples were immersed in a 5% (mass fraction) NaCl solution for corrosion testing; meanwhile another part of samples were subjected to salt spray testing. The microstructure of samples, morphology and phase constituents of corrosion products were characterized by means of field emission scanning electron microscope with energy dispersive spectrometer, 3D microscope, X-ray diffractometer. Besides, the micro-area corrosion behavior of the cut edges of different galvanized coatings was characterized by scanning electrochemical microscopy (SECM). Results show that the corrosion products are distributed both on the coating at the cut edge area and on the steel substrate near the coating. The corrosion products on the Zn and Zn-3Mg coatings were mainly simonkolleite, and on the steel substrate were mainly Zn5(OH)8Cl2 and hydrozincite (Zn5(OH)6(CO3)2). For Zn-5Al and Zn-4Al-3Mg coatings, the main corrosion products were layered double hydroxide (Zn6Al2(OH)16CO3·4H2O), Zn5(OH)8Cl2, and Zn5(OH)6(CO3)2·H2O. Scanning electrochemical microscope measurements revealed that initially, the feedback currents of Zn-Al and Zn-Al-Mg coatings were higher than those of Zn. Over time, the feedback currents of Zn-Al and Zn-Al-Mg coatings decreased to levels below those of Zn. The feedback current on the surface of the coating and the surface of the steel substrate far away from the side of the coating are larger, while the feedback current on the surface of the steel substrate close to the side of the coating is smaller. Overall, both the feedback current and the current depression decreased with the corrosion time. Salt spray corrosion tests showed that the average weight loss rate of cut edges is 1.04 × 10-2, 9.88 × 10-3, 5.73 × 10-3, and 5.21 × 10-3 g·m-1·h-1 for that with coatings of pure Zn, Zn-Mg, Zn-Al, and Zn-Al-Mg respectively. Among others, the corrosion resistance of the cut-edge with Zn-4Al-3Mg coating is the best. The corrosion product layer of Zn-4Al-3Mg coating is compact with higher content of protective products, Zn5(OH)8Cl2 and Zn6Al2(OH)16CO3·4H2O, provides a synergistic protective effect. The good protective performance of the corrosion products layer makes the Zn-Al-Mg coating show superior long-term corrosion resistance.

Key words: Zn-based eutectic alloys    corrosion products    cutting-edge corrosion    localized corrosion    localized electrochemistry    corrosion behavior
收稿日期: 2025-07-15      32134.14.1005.4537.2025.225
ZTFLH:  TG178.44  
基金资助:国家自然科学基金(52461011);广西科技计划项目(AA24263065);广西科技计划项目(AB25069311);中国博士后科学基金(2023MD744187)
通讯作者: 王友彬,E-mail:wangyoubin@gxu.edu.cn,研究方向为金属腐蚀与防护
Corresponding author: WANG Youbin, E-mail: wangyoubin@gxu.edu.cn
作者简介: 李永坤,男,1998年生,硕士生
SampleAlMgZn
Zn-3Mg alloy-3.1796.83
Zn-5Al alloy5.13-94.87
Zn-4Al-3Mg alloy4.063.1892.76
表1  所制备的锌合金化学成分
图1  镀层切边的俯视角度与浸泡示意图
图2  镀层表面的微观组织形貌
SampleSpotZnAlMgFePhase
Zn coating198.63--1.37η-Zn
298.51--1.49η-Zn
Zn-Mg coating197.34-0.821.84`η-Zn
267.11-30.442.45MgZn2
367.86-31.352.79MgZn2
Zn-Al coating192.854.89-2.26η-Zn
290.446.72-2.84η-Zn
337.4560.02-2.53β-Al
Zn-Al-Mg coating194.623.84-1.54η-Zn
292.395.18-2.43η-Zn
365.37-31.13.53MgZn2

4

77.12

12.39

7.27

3.22

η-Zn/α-Al/MgZn2 ternary eutectic
表2  图2中标记位置的EDS元素分析结果
图3  镀层切边在5%NaCl溶液中浸泡6 h后的微观组织
SampleSpotZnAlMgCl
Zn coating148.76--7.64
234.88--5.18
330.16--4.47
Zn-Mg coating150.58-1.226.69
233.98--8.06
331.17--4.20
Zn-Al coating138.2212.40-7.78
231.260.85-4.25
329.930.81-3.96
Zn-Al-Mg coating137.258.010.466.82
228.1017.45-7.71
331.450.56-6.21
表3  图3中标记位置的EDS元素分析结果
图4  在5%NaCl溶液中浸泡不同时间后不同镀层切边的腐蚀产物分布
图5  在5%NaCl溶液中浸泡不同时间后不同镀层切边处的SECM线扫描曲线
图6  在5%NaCl溶液中浸泡不同时间后不同镀层切边的SECM面扫描图
图7  盐雾腐蚀24 h后不同镀层的XRD图谱
图8  不同镀层切边样品在24 h中性盐雾试验中的平均失重速率
图9  盐雾腐蚀168 h后不同镀层的SEM截面图像及对应的EDS面扫描图
SampleSpotZnAlMgFePhase
Zn coating198.28--1.72η-Zn
292.71--7.29ζ-FeZn13
392.87--7.13ζ-FeZn13
489.14--10.86δ-FeZn10
Zn-Mg coating198.62-0.271.11η-Zn
264.64-32.512.85MgZn2
366.41-30.493.10MgZn2
488.96--11.04δ-FeZn10
Zn-Al coating185.5511.01-3.44Zn/Al binary eutectic
262.8324.57-12.60-
328.4362.21-9.36Fe2Al5Znx
Zn-Al-Mg coating133.6865.01-1.31α-Al
293.554.27-2.18η-Zn
365.09-32.172.74MgZn2
466.22-30.992.79MgZn2
527.8165.38-6.91Fe2Al5Znx
表4  图9中标记位置的EDS元素分析结果
图10  盐雾腐蚀24 h后,去除腐蚀产物后的腐蚀形貌
图11  锌合金镀层切边腐蚀过程示意图
[1] He X, Zhou X, Shang T, et al. Influence mechanism of different elements and alloy phases on the corrosion resistance of Zn-Al-Mg coated steel in the atmospheric environment: A review [J]. Corros. Commun., 2024, 13: 49
doi: 10.1016/j.corcom.2023.11.001
[2] Ding C F, Ma Z, Liu S W, et al. Research on design and microstructure of hot-dip Zn-Al-Mg/Sn alloy [J]. Mater. Charact., 2022, 185: 111746
doi: 10.1016/j.matchar.2022.111746
[3] Zhao Q, Zhang J, Mao R R, et al. Stress corrosion and its mechanism of hot-dip galvanized coating on Q235 steel structure [J]. J. Chin. Soc. Corros. Prot., 2024, 44: 1305
[3] 赵 骞, 张 洁, 毛锐锐 等. Q235钢结构件表面热镀锌层的应力腐蚀及其机理 [J]. 中国腐蚀与防护学报, 2024, 44: 1305
[4] Chaouki A, Ben Ali M, El Maalam K, et al. Optimizing corrosion protection: Performance comparison of Zn and Zn-Al-Mg alloys hot-dip galvanized coatings [J]. J. Alloy. Compd., 2024, 1007: 176371
doi: 10.1016/j.jallcom.2024.176371
[5] Gu T Z, Liu Y W, Peng C, et al. Initial atmospheric corrosion of zinc-aluminum-magnesium coated steel and galvanized steel in regions of extremely cold and industrial climate [J]. Mater. Chem. Phys., 2022, 291: 126686
doi: 10.1016/j.matchemphys.2022.126686
[6] Jiang G R, Liu G H, Shang T. Effect of heat treatment process on microstructure and corrosion resistance of ZnAlMg coating [J]. J. Chin. Soc. Corris. Prot., 2024, 44: 246
[6] 蒋光锐, 刘广会, 商 婷. 热处理对ZnAlMg镀层组织与耐腐蚀性能的影响 [J]. 中国腐蚀与防护学报, 2024, 44: 246
[7] Jiang G R, Liu G H. Microstructure and corrosion resistance of solidified Zn-Al-Mg alloys [J]. J. Chin. Soc. Corros. Prot., 2018, 38: 191
[7] 蒋光锐, 刘广会. Zn-Al-Mg合金的凝固组织及其耐腐蚀性能 [J]. 中国腐蚀与防护学报, 2018, 38: 191
doi: 10.11902/1005.4537.2017.022
[8] Gu T Z, Liu Y W, Peng C, et al. Corrosion behavior of hot-dip Zn-Al-Mg coating exposed to a simulated hot and humid marine atmosphere [J]. Surf. Technol., 2024, 53(2): 110
[8] 顾天真, 刘雨薇, 彭 灿 等. 热浸镀Zn-Al-Mg镀层在模拟湿热海洋大气环境中的腐蚀行为研究 [J]. 表面技术, 2024, 53(2): 110
[9] Volovitch P, Vu T N, Allély C, et al. Understanding corrosion via corrosion product characterization: II. Role of alloying elements in improving the corrosion resistance of Zn-Al-Mg coatings on steel [J]. Corros. Sci., 2011, 53: 2437
doi: 10.1016/j.corsci.2011.03.016
[10] Zhong X Z, Wang Z Y, Liu Y J, et al. Corrosion behavior of galvanized steel in simulated ocean atmosphere [J]. J. Chin. Soc. Corros. Prot., 2015, 35: 151
[10] 钟西舟, 王振尧, 刘艳洁 等. 镀锌钢在模拟海洋大气环境下的腐蚀行为 [J]. 中国腐蚀与防护学报, 2015, 35: 151
doi: 10.11902/1005.4537.2014.081
[11] Persson D, Thierry D, Karlsson O. Corrosion and corrosion products of hot dipped galvanized steel during long term atmospheric exposure at different sites world-wide [J]. Corros. Sci., 2017, 126: 152
doi: 10.1016/j.corsci.2017.06.025
[12] Persson D, Thierry D, Lebozec N. The effect of microstructure on local corrosion product formation during initial SO2-induced atmospheric corrosion of ZnAlMg coating studied by FTIR-ATR FPA chemical imaging [J]. Corros. Mater. Degrad., 2023, 4: 503
doi: 10.3390/cmd4030026
[13] Thierry D, Persson D, Luckeneder G, et al. Atmospheric corrosion of ZnAlMg coated steel during long term atmospheric weathering at different worldwide exposure sites [J]. Corros. Sci., 2019, 148: 338
doi: 10.1016/j.corsci.2018.12.033
[14] Yang X R, Wang J H, Ren Z X, et al. Preparation and corrosion resistance of Ni-Fe layer double hydroxides superhydrophobic film on carbon steel [J]. Colloids Surf., 2023, 669A: 131501
[15] Jing C, Dong B Q, Raza A, et al. Corrosion inhibition of layered double hydroxides for metal-based systems [J]. Nano Mater. Sci., 2021, 3: 47
[16] Yuan X H, Lin Y, Zhang Q F. Cut-edge protection performance and corrosion resistance mechanisms of galvanized Zn-Al-Mg alloy coating [J]. Chin. J. Nonferrous Met., 2015, 25: 2453
[16] 袁训华, 林 源, 张启富. 热镀锌铝镁镀层的切边保护性能和耐腐蚀机理 [J]. 中国有色金属学报, 2015, 25: 2453
[17] Yasakau K A, Kallip S, Lisenkov A, et al. Initial stages of localized corrosion at cut-edges of adhesively bonded Zn and Zn-Al-Mg galvanized steel [J]. Electrochim. Acta, 2016, 211: 126
doi: 10.1016/j.electacta.2016.06.045
[18] Lee J W, Park B R, Oh S Y, et al. Mechanistic study on the cut-edge corrosion behaviors of Zn-Al-Mg alloy coated steel sheets in chloride containing environments [J]. Corros. Sci., 2019, 160: 108170
doi: 10.1016/j.corsci.2019.108170
[19] Azevedo M S, Allély C, Ogle K, et al. Corrosion mechanisms of Zn(Mg, Al) coated steel in accelerated tests and natural exposure: 1. The role of electrolyte composition in the nature of corrosion products and relative corrosion rate [J]. Corros. Sci., 2015, 90: 472
doi: 10.1016/j.corsci.2014.05.014
[20] Prosek T, Nazarov A, Le Gac A, et al. Coil-coated Zn-Mg and Zn-Al-Mg: Effect of climatic parameters on the corrosion at cut edges [J]. Prog. Org. Coat., 2015, 83: 26
[21] Lee J W, Son I, Kim S J. Newly designed surface control using Si addition in trace quantity for Zn-2Al-3Mg alloy coated steel sheet with improved corrosion resistance [J]. Appl. Surf. Sci., 2022, 598: 153868
doi: 10.1016/j.apsusc.2022.153868
[22] Oh M S, Kim S H, Kim J S, et al. Surface and cut-edge corrosion behavior of Zn-Mg-Al alloy-coated steel sheets as a function of the alloy coating microstructure [J]. Met. Mater. Int., 2016, 22: 26
doi: 10.1007/s12540-015-5411-9
[23] Tokuda S, Nishida Y, Nishimoto M, et al. Initial dissolution of Mg-containing phase and corrosion product formation in cut-edge corrosion of Zn-11%Al-3%Mg-0.2%Si coated steel [J]. Corros. Sci., 2023, 225: 111605
doi: 10.1016/j.corsci.2023.111605
[24] Suzuki Y, Yamaguchi S, Matsumoto M, et al. Mechanism of corrosion protection at cut edge of Zn-11%Al-3%Mg-0.2%Si coated steel sheets [J]. ISIJ Int., 2020, 60: 2038
doi: 10.2355/isijinternational.ISIJINT-2019-765
[25] Zhou W J, Xu L K, Wang J, et al. Corrosion electrochemical behavior of Zn-Al silane coating on carbon steel [J]. Acta Metall. Sin., 2007, 43: 983
[25] 周文娟, 许立坤, 王 佳 等. 碳钢表面硅烷锌铝涂层的腐蚀电化学行为 [J]. 金属学报, 2007, 43: 983
[26] Skaanvik S A, Gateman S M. Probing passivity of corroding metals using scanning electrochemical probe microscopy [J]. Electrochem. Sci. Adv., 2024, 4: e2300014
doi: 10.1002/elsa.v4.5
[27] Wang L W, Li X G, Du C W, et al. Recent advances in local electrochemical measurement techniques and applications in corrosion research [J]. J. Chin. Soc. Corros. Prot., 2010, 30: 498
[27] 王力伟, 李晓刚, 杜翠薇 等. 微区电化学测量技术进展及在腐蚀领域的应用 [J]. 中国腐蚀与防护学报, 2010, 30: 498
[28] Feng J Q, Wang Y B, Lin X L, et al. SECM in situ investigation of corrosion and self-healing behavior of trivalent chromium conversion coating on the zinc [J]. Surf. Coat. Technol., 2023, 459: 129411
doi: 10.1016/j.surfcoat.2023.129411
[29] Traxler I, Singewald T D, Schimo-Aichhorn G, et al. Scanning electrochemical microscopy methods (SECM) and ion-selective microelectrodes for corrosion studies [J]. Corros. Rev., 2022, 40: 515
doi: 10.1515/corrrev-2021-0104
[30] Wang X Y, Xia Y, Zhou Y R, et al. Corrosion behavior of pure mg based on generation/collection and feedback modes of scanning electrochemical microscopy [J]. Acta Metall. Sin., 2015, 51: 631
doi: 10.11900/0412.1961.2014.00602
[30] 王新印, 夏 妍, 周亚茹 等. 基于扫描电化学显微镜产生/收集和反馈模式研究纯Mg腐蚀行为 [J]. 金属学报, 2015, 51: 631
doi: 10.11900/0412.1961.2014.00602
[31] Amemiya S, Bard A J, Fan F R F, et al. Scanning electrochemical microscopy [J]. Annu. Rev. Anal. Chem, 2008, 1: 95
doi: 10.1146/anchem.2008.1.issue-1
[32] Zoski C G. Review—Advances in scanning electrochemical microscopy (SECM) [J]. J. Electrochem. Soc., 2016, 163: H3088
doi: 10.1149/2.0141604jes
[33] Lin X L, Wang Y B, Xin Y C, et al. Localized electrochemical corrosion behavior of the interface of hot-dip galvanized coating [J]. Surf. Technol., 2022, 51(9): 217
[33] 林学亮, 王友彬, 辛延琛 等. 热浸镀锌层界面的微区电化学腐蚀行为 [J]. 表面技术, 2022, 51(9): 217
[34] Lin Y, Liu T, Guo Y B, et al. Research and development of welding materials for low-temperature steel and corrosion evaluation methods [J]. J. Chin. Soc. Corros. Prot., 2024, 44: 957
[34] 林 一, 刘 涛, 郭彦兵 等. 船用低温钢焊接材料的研发与腐蚀方法评价 [J]. 中国腐蚀与防护学报, 2024, 44: 957
[35] Wang J, Ning P D, Liu Q Q, et al. Corrosion behavior of galvanized steel in a simulated marine atmospheric environment [J]. J. Chin. Soc. Corros. Prot., 2023, 43: 578
[35] 王 瑾, 宁培栋, 刘倩倩 等. 模拟海洋大气环境中镀锌钢的腐蚀行为和机理 [J]. 中国腐蚀与防护学报, 2023, 43: 578
[1] 赵密锋, 胡芳婷, 刘艳明, 宋文文, 谢俊峰, 吕祥鸿, 代盼, 胡航波. 含氧注气驱高Ca2+ 浓度工况下C110钢腐蚀产物膜演变及腐蚀行为研究[J]. 中国腐蚀与防护学报, 2026, 46(3): 821-832.
[2] 冯晨旭, 崔腾飞, 徐璐, 张昕宇, 崔中雨. A588耐候钢在极寒大气环境下的腐蚀行为研究[J]. 中国腐蚀与防护学报, 2026, 46(3): 875-882.
[3] 贺佳, 李欢, 覃世军, 芦伟, 汪卫华, 储德林. 高温流动液态锂铅对氧化物弥散强化钢的长时间腐蚀行为研究[J]. 中国腐蚀与防护学报, 2026, 46(3): 911-918.
[4] 陈旭, 杨浩, 田一晨, 张国庆, 宋博, 王岐山, 肖成灿. D36低碳钢在不同模拟海洋环境中初期腐蚀行为研究[J]. 中国腐蚀与防护学报, 2026, 46(2): 549-557.
[5] 王乙初, 刘天龙, 张思倩, 赵利, 骆智超, 郑开宏. 含V、W高Mn奥氏体耐热钢在熔融Na2SO4 中的热腐蚀行为[J]. 中国腐蚀与防护学报, 2026, 46(2): 620-628.
[6] 戴念维, 窦欣懿, 刘华剑, 冷滨. 增材制造合金在核能领域应用中的腐蚀研究进展[J]. 中国腐蚀与防护学报, 2026, 46(1): 15-24.
[7] 杨潇文, 陈泽浩, 杨莎莎, 王群昌, 王金龙, 陈明辉, 王福会. 镍基单晶高温合金N5及其纳米晶涂层的短期热腐蚀行为研究[J]. 中国腐蚀与防护学报, 2026, 46(1): 252-260.
[8] 蔡科涛, 季磊, 张震, 冯强, 邓伟林, 兰贵红, 何莎, 赵占勇, 白培康. Mg-Gd-Y-Zn-Zr合金在NaCl和Na2SO4 溶液中腐蚀行为研究[J]. 中国腐蚀与防护学报, 2025, 45(5): 1289-1299.
[9] 冯宇芹, 郭同翰, 余韦汉, 吴伟, 张大全. Sb对高强结构钢在东海环境中腐蚀行为的影响[J]. 中国腐蚀与防护学报, 2025, 45(5): 1300-1308.
[10] 谷松伦, 张繁, 黄国胜, 姜丹, 董国君. 冷喷涂Cu-Ti伪合金防污材料的腐蚀行为[J]. 中国腐蚀与防护学报, 2025, 45(5): 1309-1319.
[11] 罗铸, 刘佳乐, 魏安超, 黄洪林, 李鑫, 于延钊, 张梦飞. 高温高CO2 压力下低合金钢P110SS在氯盐和甲酸盐溶液中腐蚀行为对比研究[J]. 中国腐蚀与防护学报, 2025, 45(5): 1390-1398.
[12] 范世林, 杜娟, 杨少丹, 周延军, 宋克兴, 张国赏, 岳鹏飞, 杨冉, 王晓军. Cu-15Ni-8Sn合金在含S2- 的3.5%NaCl溶液中的腐蚀行为[J]. 中国腐蚀与防护学报, 2025, 45(5): 1408-1416.
[13] 黄诗雨, 刘士琛, 杨淞普, 刘家兵, 李刚, 郭娜, 刘涛. FH40船用钢在模拟极地海水环境中的腐蚀与磨蚀行为[J]. 中国腐蚀与防护学报, 2025, 45(4): 859-868.
[14] 段敬民, 董勇, 缪东美, 杨玉婧, 毛凌波, 章争荣. 热处理工艺对Al0.5CoCrFeNi高熵合金在不同介质下腐蚀行为及力学性能的影响[J]. 中国腐蚀与防护学报, 2025, 45(4): 983-994.
[15] 张珊珊, 刘元才, 徐铁伟, 杨发展. 成型方向及热处理对选区激光熔化Ti6Al4V合金腐蚀性能的影响[J]. 中国腐蚀与防护学报, 2025, 45(4): 995-1004.