中国腐蚀与防护学报  2002, Vol. 22 Issue (1): 48-53          
  研究报告 本期目录 | 过刊浏览 |
用丝束电极研究SRB微生物诱导腐蚀的电化学特征
董泽华;郭兴蓬;刘宏芳
武汉华中科技大学化学系
STUDY ON ELECTROCHEMISTRY CHARACTERISTICSIN MIC BY WIRE BEAM ELECTRODES
Zehua Dong;Xingpeng Guo;Hongfang Liu
武汉华中科技大学化学系
引用本文:

董泽华; 郭兴蓬; 刘宏芳 . 用丝束电极研究SRB微生物诱导腐蚀的电化学特征[J]. 中国腐蚀与防护学报, 2002, 22(1): 48-53 .
, , . STUDY ON ELECTROCHEMISTRY CHARACTERISTICSIN MIC BY WIRE BEAM ELECTRODES[J]. J Chin Soc Corr Pro, 2002, 22(1): 48-53 .

全文: PDF(185 KB)  
摘要: 应用丝束电极研究了半连续培养基中SRB及其生物膜对Q235 低碳钢腐蚀的影响.采用电位、电流以及阻抗扫描技术测试了生物膜的不均匀性特性,以及 电极开路电位和电化学阻抗谱(EIS)与培养时间的关系.发现随生物膜的成长,开路电位负 移.由于生物膜中SRB代谢产生的硫化物具有导电性,使表面电位扫描已不能作为生物膜下 局部腐蚀的判据,但表面阻抗扫描却可探测到膜下的局部腐蚀.EIS表明,生物膜电容极大( 104~105 μF/cm2),且膜电容随时间呈S型增加,而溶液电阻和电荷传递电阻则呈指 数下降.
关键词 : 微生物诱导腐蚀,  碳钢,  电化学阻抗谱    
Abstract:Wire beam electrode(WBE) was applied to study the m icrobiologically influenced corrosion(MIC) of Q235 carbon steel associated with sulphate reducing bacteria(SRB) in semicontinuous culture medium(to be complete ly refreshed every 72 hours).The potential,galvanic current density and impedanc e mapping,as well as open circuit potential(OCP) and electrochemical impedance s pectrum(EIS) were measured to predict the localized corrosion under biofilm duri ng SRB growing.As a result,the OCP moved negatively gradually with time.However, The mapping showed the potential fluctuation on the WBE surface decreased over t ime due to the conductivity of FeSx(x=0.9~2) metabolized by SRB in th e biofilm.Therefore,the potential mapping could not be a criterion of localized corrosion under biofilm.Instead,the impedance mapping could give a good predicti on to the MIC.In addition,The biofilm capacity moved up to a very large level(~ 105 μF/cm2) in shape of sigmoid when SRB grew.At the same time,both solutio n resi〖JP2〗stance and charge transfer resistance decreased exponentially.〖JP 〗
Key words: microbiologically influenced corrosion    carbon steel    electrochemical impedance spectrum
收稿日期: 2000-10-08     
ZTFLH:  TG174  
[1]DanielH ,PopeE ,AlanMorrisIII.Someexperienceswithmicrobi ologicallyinfluencedcorrosionofpipelines[J].MaterialsPerfor mance,1995,34(5):23-28
[2]SoebbingJohnB ,YoloRogerA .Microbiologicallyinfluencedcorro sioninwastewatertreatmentplants[J].MaterialsPerformance,1996,35(9):41-48
[3]GeorgeJLicina,CurtisSCarnery.MonitoringbiofilmformationandincipientMICinrealtime[A].Corrosion99,NACE[C].Hous ton,TX ,1999,175
[4]FranklinMichaelJ ,WhiteDavidC ,IsaacsHughS .Pittingcorrosionbybacteriaoncarbonsteeldeterminedbythescanningvibratingelectrodetechnique[J].Corros.Sci.,1991,32(9):945-952
[5]FranklinMJ,NivensDE ,GuckertJB .Effectofelectrochemicalimpedancespectroscopyonmicrobialbiofilmscellnumbers,viabilityandactivity[J].Corrosion,1991,47(7):519-522
[6]TanYJ .Monitoringlocalizedcorrosionprocessesandestimatinglo calizedcorrosionratesusingawirebeamelectrode[J].Corrosion,1998,54(5):403~413
[7]TanYongjun.Wirebeamelectrode:anewtoolforstudyinglocalizedcorrosionandotherheterogeneouselectrochemicalprocesses[J].Corros.Sci.,1999,41(2):229~247
[8]MansfeldFlorian,etal.Technicalreviewofelectrochemicaltech niquesappliedtomicrobiologicallyinfluencedcorrosion[J].Corros.Sci.,1991,32(3):242-272
[9]PengCG ,ParkJK .Principalfactorsaffectingmicrobiologicallyin fluencedcorrosionofcarbonsteel[J].Corrosion,1994,50(9):669-675
[10]ChungY ,ThomasLK .ComparisonofMICpitmorphologywithnon-micchlorideinducedpitsintype304/304L/E308stainlesssteelbasemetal/welds[A].Corrosion99,NACE [C].Houston,TX ,1999,159
[11]AngellP ,UrbanicK .Sulfate-reducingbacterialactivityasapa rametertopredictlocalizedcorrosionofstainlessalloys[J].Corros.Sci.,2000,42(5):897-912
[12]FerrerIJ,CaballeroF ,DelasHerasC ,SanchezC .Preparationofn-typedopedFeS2 thinfilms[J].SolidStateCommunications,1994,89(4):349-352
[13]CaoCN .CorrosionElectrochemistry,ThesaurusofCorrosionandProtection[M].Beijing:ChemistryIndustryPress,1994,94
(曹楚南.腐蚀电化学,腐蚀与防护全书.北京:化学工业出版社,1994,94)
[14]MacDonaldDD .TechniquesforCharacteristicofElectrodesandElectrochemicalProcess[M].EditedbyRaviVarma,SelmanJR ,NewYork:JohnWiley&Sons,1991.
[1] 谢敬礼, 王友志, 乔书振, 牛佳雨, 郝龙, 曹胜飞, 王俭秋. 高放废物地质处置库近场环境中碳钢腐蚀产物演化研究进展[J]. 中国腐蚀与防护学报, 2026, 46(5): 1343-1352.
[2] 黄胡灵彤, 王成, 程学群, 杨小佳, 张占武, 黎亮. Q235碳钢在模拟南疆土壤中的腐蚀行为[J]. 中国腐蚀与防护学报, 2026, 46(5): 1595-1604.
[3] 吴昉赟, 乔睿鑫, 李旭宁, 尚浩杰, 陆丰华, 周澄, 王欣, 董亮. 管道内海水流动特性对碳钢阴极保护影响的试验与数值模拟研究[J]. 中国腐蚀与防护学报, 2026, 46(4): 1081-1094.
[4] 魏旭光, 王维斌, 李康, 张灿灿, 吴玉庭, 鹿院卫, 王国强, 赵博. Q345R碳钢在Hitec高温熔盐中动态腐蚀特性实验对比研究[J]. 中国腐蚀与防护学报, 2026, 46(3): 693-702.
[5] 汪崧, 刘学武, 赵健, 李众, 杨吉可. 金银花植物提取物作为环保型缓蚀剂对低碳钢酸性溶液腐蚀的缓蚀效果[J]. 中国腐蚀与防护学报, 2026, 46(2): 541-548.
[6] 胡宗武, 刘建国, 王钰, 李楷. 含砂3.5%NaCl溶液中90°弯管冲刷腐蚀损伤机制研究[J]. 中国腐蚀与防护学报, 2026, 46(2): 611-619.
[7] 岳远广, 尹志彪, 张子月, 江社明, 张启富. 一种大气腐蚀实时监测装置的开发及其在不同环境中的应用[J]. 中国腐蚀与防护学报, 2026, 46(1): 308-314.
[8] 李兆南, 侯禹岑, 莒鹏, 庄铁钢, 陈景杰, 王明昱, 徐云泽. 模拟液滴电导率变化对碳钢大气腐蚀的影响机制研究[J]. 中国腐蚀与防护学报, 2025, 45(6): 1537-1548.
[9] 王得, 张璠, 王兴奇, 张贺新, 赵成志, 杨延格. 单组分氟碳改性环氧涂层对碳钢和铝合金长期防腐性能的对比研究[J]. 中国腐蚀与防护学报, 2025, 45(6): 1549-1562.
[10] 彭立园, 谢敬礼, 曹胜飞, 谭季波, 吴欣强, 张兹瑜. 日本高放废物处置容器腐蚀厚度设计研究进展[J]. 中国腐蚀与防护学报, 2025, 45(3): 563-576.
[11] 王刚, 李昭, 王涛, 段腾, 杜翠薇. 光伏桩基用钢在新疆土壤中的腐蚀行为研究[J]. 中国腐蚀与防护学报, 2024, 44(4): 987-992.
[12] 王长罡, DANIEL Enobong Felix, 李超, 董俊华, 杨华, 张东玖. 海洋环境中碳钢和不锈钢螺栓紧固件的腐蚀机制差异研究[J]. 中国腐蚀与防护学报, 2023, 43(4): 737-745.
[13] 郝文魁, 陈新, 徐玲铃, 韩钰, 陈云, 黄路遥, 祝志祥, 杨丙坤, 王晓芳, 张强. 电网碳钢、镀锌钢大气腐蚀等级图绘制研究[J]. 中国腐蚀与防护学报, 2023, 43(4): 795-802.
[14] 邹文杰, 丁立, 张雪姣, 陈均. 环氧树脂/有机硅氧烷改性阳离子丙烯酸乳液复合涂层的研究[J]. 中国腐蚀与防护学报, 2023, 43(4): 922-928.
[15] 夏晓健, 万芯媛, 陈云翔, 韩纪层, 陈奕扬, 严康骅, 林德源, 陈天鹏, 左晓梅, 孙宝壮, 程学群. 两种热处理工艺对3Cr钢腐蚀行为影响及机理研究[J]. 中国腐蚀与防护学报, 2023, 43(3): 656-662.