新型Al-Cu-Li-(Sc+Zr)合金的剥蚀行为
梁文杰;潘清林;李运春;何运斌;李文斌;周迎春;路聪阁
中南大学材料科学与工程学院 长沙 410083
EXFOLIATION CORROSION BEHAVIORS OF Al-Cu-Li-(Sc+Zr) ALLOY
LIANG Wenjie;PAN Qinglin;LI Yunchun;HE Yunbin;LI Wenbin;ZHOU Yingchun;LU Congge
School of Materials Science and Engineering; Central South University; Changsha 410083
全文: PDF(1682 KB)  
摘要: 

研究了一种新型Al-Cu-Li-(Sc+Zr)合金在不同时效状态下的剥蚀行为。结果表明:合金在自然时效状态下具有较好的抗剥落腐蚀能力, 在160 ℃下时效,随着时效时间的延长,合金剥落腐蚀敏感性逐渐增加。透射电镜(TEM)观察发现:合金主要析出相为T1 相;随着时效时间延长,T1相逐渐粗化,在晶界处还会出现无沉淀析出带(PFZ)及平衡相。合金腐蚀对比实验后,TEM微观腐蚀形貌表明,T1相和PFZ是引起合金剥蚀敏感性的主要因素,腐蚀从T1相的溶解开始,中、后期则以PFZ的溶解为主。

 

关键词 时效铝锂合金剥蚀透射电镜    
Abstract

Exfoliation corrosion behavior of Al-Cu-Li-(Sc+Zr) alloy with different aging treatment schemes were studied. The results show that the naturally-aged alloy has the best exfoliation corrosion resistance. The exfoliation corrosion are accelerated with prolonging the aging time at 160℃. Microstructure observations showed that the main precipitate of alloy is T1 phase. With increasing the aging time, T1 phase coarsened, and precipitate-free-zone (PFZ) and equilibrium phases were observed along grain boundaries. The exfoliation corrosion behaviors of Al-Cu-Li-(Sc+Zr) alloys were investigated through TEM. It is shown that T1 phase and PFZ are the main factors for the exfoliation corrosion behavior of the alloy. The corrosion of the alloy begins with the dissolution of T1 followed by the dissolution of PFZ.

Key wordsaging    Al-Li alloy    exfoliation corrosion    TEM
收稿日期: 2007-03-28     
ZTFLH: 

TG174.3

 
基金资助:

国家高技术发展计划项目(2006AA03Z523)

通讯作者: 潘清林     E-mail: pql@mail.csu.edu.cn
Corresponding author: PAN Qinglin     E-mail: pql@mail.csu.edu.cn

引用本文:

梁文杰 潘清林 李运春 何运斌 李文斌 周迎春 路聪阁. 新型Al-Cu-Li-(Sc+Zr)合金的剥蚀行为[J]. 中国腐蚀与防护学报, 2009, 29(1): 30-34.
HU Dao-Chun, XUN Le-Min, SHANG Guan-Bao. EXFOLIATION CORROSION BEHAVIORS OF Al-Cu-Li-(Sc+Zr) ALLOY. J Chin Soc Corr Pro, 2009, 29(1): 30-34.

链接本文:

https://www.jcscp.org/CN/      或      https://www.jcscp.org/CN/Y2009/V29/I1/30

[1] Yin D F,Zheng Z Q. History and current status of Al-Li alloys research and development[J].Mater. Rev., 2003,17(2):18-20
(尹登峰,郑子樵.铝锂合金研究开发的历史与现状[J]. 材料导报,2003,17(2):18-20)
[2] Qiu H Z,Wu Z H. Development of aerospace materials abroad[J]. Aerospace Mater. Technol.,1997,1(4):5-13
(邱惠中,吴志红.国外航天材料的新进展[J]. 宇航材料工艺,1997,1(4):5-13)
[3] Tian R Z,Wang Z T. Processing of Aluminum Alloy[M]. Changsha:Central South University Press,2000
(田荣璋,王祝堂. 铝合金及其加工手册[M]. 长沙:中南大学出版社,2000)
[4] He J P,Chen W L,Xu W,et al. Effect of exfoliation on structure and tensile strength of LC4CS aluminum alloy at constant temperature[J]. Trans.Nanjing Univ. Aeronaut. Astronaut.,1999,31(5):575-579
(何建平,陈文理,许玮等.恒温剥蚀对LC4CS铝合金结构和力学性能的影响[J]. 南京航空航天大学学报,1999,31(5):575-579)
[5] Li J F,Cao F H,Zhang Z,et al. Review on exfoliation susceptibility of aluminium alloys and quantitative measurement method[J]. J. Chin. Soc. Corros.Prot.,2004,24 (1) : 55-58
(李劲风,曹发和,张昭等. 铝合金剥蚀敏感性及其定量研究方法[J]. 中国腐蚀与防护学报,2004,24 (1):55-58)
[6] Zhou C R,Pan Q L,Zhu C M,et al. Development and study of new types aluminum-lithium alloys[J]. Mater. Rev.,2004,26(6):70-75
(周昌荣,潘青林,朱朝明等. 新型铝锂合金的研究和进展[J]. 材料导报,2004,26(6):70-75)
[7] Wang X Y,Pan Q L,Zhou C R,et al. Recent situation and development trend of Sc containing Al-Li alloy[J]. Chinese Rare Earths,2005,26(6):70-75
(王新宇,潘青林,周昌荣等. 含钪铝锂合金的研究与发展[J]. 稀土,2005,26(6):70-75)
[8] ASTM G34-2001. Standard test method for exfoliation corrosion susceptibility in 2XXX and 7XXX. series aluminium alloys[S].
[9] Su J X,Zhang Z,Cao F H,et al. Review on the intergranular corrosion and exfoliation corrosion of aluminum alloys[J]. J. Chin. Soc. Corros. Prot.,2005,25(3):187-192
(苏景新,张昭,曹发和等. 铝合金的晶间腐蚀与剥蚀[J]. 中国腐蚀与防护学报,2005,25(3):187-192)
[10] Iwamura S,Nakayama M,Miura Y. Coherency between Al3Sc precipitate and the matrix in Al alloys containing Sc[J]. Mater. Sci. Forum,2002,396-402:1151-1156
[11] Buchheit R G,Moran J P,Stoner G E. Localized corros- ion behavior of alloy 2090 the role of microstructure heterogeneity[J]. Corrosion,1990,46(8):610-617
[12] Kumai C,Kusinski J,Thomas G. Influence of aging at 200℃ on the corrosion resistance of Al-Li and Al-Cu-Li alloys[J]. Corrosion,1989,45(4):294-302
[13] Wall F D,Stoner G E. The evaluation of the critical ele- ctrochemical potentials influencing environmentally assisted cracking of Al-Li-Cu alloys in selected environments[J]. Corros.Sci.,1997,39(5):835-853
[14] Wei X Y,Tan C Y,Zheng Z Q. Influence of aging on corr- osion behavior of 2195 Al-Li alloy[J]. Chin. J. Nonferrous. Met.,2004,14(7):1195-1200
(魏修宇,谭澄宇,郑子樵. 时效对2195铝锂合金腐蚀行为的影响[J]. 中国有色金属学报,2004,14(7):1195-1200)
[15] Li G H. Microstructure of 8090 Al-Li alloys welded jo- int[A]. Proceedings of the First National Symposium on Al-Li Alloys [C]. Shenyang,1991
(李敢红. 8090铝锂合金焊接接头微观组织[A]. 第一届全国铝锂合金研讨会论文集[C].沈阳,1991)
[16]  Li J F,Zheng Z Q,Ren W D. Function mechanism of seco- ndary phase on localized corrosion of Al alloy[J]. Mater. Rev.,2005,19(2):81-83
(李劲风,郑子樵,任文达. 第二相在铝合金局部腐蚀中的作用机制[J]. 材料导报,2005,19(2):81-83)

[1] 武栋才,韩培德. 中温时效处理对SAF2304双相不锈钢耐蚀性的影响[J]. 中国腐蚀与防护学报, 2020, 40(1): 51-56.
[2] 肖金涛,陈妍,邢明秀,鞠鹏飞,孟引根,王芳. 工艺参数对2195铝锂合金阳极氧化膜的耐蚀性影响[J]. 中国腐蚀与防护学报, 2019, 39(5): 431-438.
[3] 于美,魏新帝,范世洋,刘建华,李松梅,钟锦岩. 应力作用下2297铝锂合金腐蚀行为研究[J]. 中国腐蚀与防护学报, 2019, 39(5): 439-445.
[4] 任建平,宋仁国. 双级时效对7050铝合金力学性能及氢脆敏感性的影响[J]. 中国腐蚀与防护学报, 2019, 39(4): 359-366.
[5] 刘丹阳, 汪洁霞, 李劲风, 陈永来, 张绪虎, 许秀芝, 郑子樵. Mg,Ag,Zn微合金化Al-Cu-Li系铝锂合金T6态时效的晶间腐蚀行为[J]. 中国腐蚀与防护学报, 2018, 38(2): 183-190.
[6] 逄旭光, 刘润青, 王文涛, 史艳华, 李飞, 梁平. 时效温度对S32750超级双相不锈钢组织和抗氢氟酸腐蚀性能的影响[J]. 中国腐蚀与防护学报, 2017, 37(6): 519-525.
[7] 宋丰轩,赵启忠,李飞龙,任月路,黄奎,张新明. 不同时效态7050铝合金板材腐蚀速率测量[J]. 中国腐蚀与防护学报, 2017, 37(3): 287-292.
[8] 苏艳,张伦武,钟勇. 5A90铝锂合金显微组织及海洋大气环境腐蚀行为[J]. 中国腐蚀与防护学报, 2016, 36(3): 260-266.
[9] 王永霞, 向红亮, 杨彩萍, 刘东. 含铜双相不锈钢在无菌/含菌环境下的耐蚀性研究[J]. 中国腐蚀与防护学报, 2014, 34(6): 558-565.
[10] 许龙, 姚希, 李劲风, 蔡超. 2099铝锂合金晶间腐蚀行为与时效制度的相关性[J]. 中国腐蚀与防护学报, 2014, 34(5): 419-425.
[11] 华小珍, 黄晋华, 聂轮, 周贤良, 彭新元. 时效温度对15-5PH不锈钢组织及耐蚀性的影响[J]. 中国腐蚀与防护学报, 2014, 34(2): 131-137.
[12] 赵 凯 尹志民 段佳琦 邓 英. 时效处理工艺对1975合金腐蚀性能的影响[J]. 中国腐蚀与防护学报, 2013, 33(2): 153-158.
[13] 张雨,王均,石树坤,王院生. 时效对2205双相不锈钢在硫环境下的电化学腐蚀行为[J]. 中国腐蚀与防护学报, 2012, 32(6): 496-500.
[14] 谭季波,吴欣强,韩恩厚. 动态应变时效对核电材料环境致裂影响的研究现状与进展[J]. 中国腐蚀与防护学报, 2012, 32(6): 437-442.
[15] 赵义,王福. 热处理工艺对17-4PH钢耐海水腐蚀性能的影响[J]. 中国腐蚀与防护学报, 2011, 31(6): 473-477.