人造水晶釜开裂的研究
郑文龙
上海材料研究所
THE FRACTURE BEHAVIOUR OF PRESSURE VESSELS FOR GROWTH OF CULURED QUARTZ CRYSTALS
Zheng Menlong (Shanghai Research Institute of Materials)
全文: PDF(2485 KB)  
摘要: 本文从两个实际人造水晶釜开裂形态观察及产物分析入手,研究丁CrNiMo低合金高强度钢在NaOH,水溶液中SCC及CF行为,提出人造水晶釜开裂的类型、机理及提高抗断裂能力的途径。试验结果还表明对CrNiMo低合金钢-NaOH水溶液体系,CF过程中的SCC行为可以降低CF裂纹扩展速率。
Abstract:In this paper the fractography and corrosion product analysis of fractured pressure vessels for growth of cultured quartz crystals were analysed, and the behaviour of stress corrosion cracking(SCC), corrosion fatigue(CF) of CrNiMo low alloy steels in NaOH solution were investigated systematically. The results reveal that the fracture of pressure vessels for growth of cultured quartz crystals is caused by CF. For the CrNiMo low alloy steel-NaOH solution system, a platen was observed in the da/dn versus ΔK curves, but the mechanism does not to SCC, the da/dN in the second stage of CF is reduced by SCC in CF process.
收稿日期: 1987-02-25     

引用本文:

郑文龙. 人造水晶釜开裂的研究[J]. 中国腐蚀与防护学报, 1987, 7(1): 41-49.
. THE FRACTURE BEHAVIOUR OF PRESSURE VESSELS FOR GROWTH OF CULURED QUARTZ CRYSTALS. J Chin Soc Corr Pro, 1987, 7(1): 41-49.

链接本文:

https://www.jcscp.org/CN/      或      https://www.jcscp.org/CN/Y1987/V7/I1/41

[1] Papen, P.L., Pressure Vessels for Growth of Cultured Quartz Crystals, No. 61-GP 99-008, National Forge Company, February.,1, 4 (1974)
[2] 人工晶体所,φ250-2~#高压釜的设计与失效,(1982)
[3] 北京钢铁研究总院,高压釜破断事故分忻,9(1982)
[4] 北京重型机器厂.φ5250_2-80-3~#高压釜失效分析报告.4 (1983)
[5] 郑文龙;朱国培;蔡安定;人造水晶高压釜开裂分析.11(1983)
[6] 高桥克;熊谷义一;压力技术,19,1,(1981)
[7] 郑文龙;蔡安定;朱国培;金属学报,19(2) ,A134(1983)
[8] Wei, R. P.; Landes, J. D., Met. Res Standard, 9, 25(1969)
[9] Austen, J. M.; Walker E. F; I. Mech. E. Conference Publicatlons, 4, 1 (1977)
[10] 肖纪美,金属材料研究,3 (2) ,181 (1975)
No related articles found!