模拟海洋大气环境下冲刷载荷对Q355钢的腐蚀规律研究
钟振坤, 关蕾, 傅汉龙, 王俊, 刘淼然, 揭敢新

Corrosion Behavior of Q355 Steel Under Erosion Load in a Simulated Marine Atmospheric Environment
ZHONG Zhenkun, GUAN Lei, FU Hanlong, WANG Jun, LIU Miaoran, JIE Ganxin
表4 Q355钢在有无冲刷下动极化电化学参数
Table 4 Electrochemical parameters of dynamic polarization of Q355 steel under stagnant and flowing conditions
NameEcorr vs.SCE / VIcorr / A·cm-2βa / mV·dec-1βc / mV·dec-1
N0-0.70 ± 0.088.5 ± 2.777.29 ± 3.22-62.12 ± 5.12
N1-0.72 ± 0.11525 ± 18230.34 ± 4.21-121.32 ± 0.08
N2-0.69 ± 0.04590 ± 31271.98 ± 19.06-121.88 ± 1.15
N3-0.68 ± 0.03456 ± 8237.66 ± 10.93-124.45 ± 0.05
N4-0.52 ± 0.02300 ± 27201.56 ± 10.24-147.95 ± 0.06
F1-0.65 ± 0.02612 ± 23248.78 ± 12.41-115.50 ± 1.53
F2-0.58 ± 0.05902 ± 73234.48 ± 6.59-123.75 ± 3.82
F3-0.49 ± 0.04501 ± 27201.04 ± 4.30-157.19 ± 2.89
F4-0.47 ± 0.03337 ± 22189.41 ± 10.12-153.33 ± 7.08