FeCrAl表面氧化对氘渗透性能影响研究
高士鑫, 尹春雨, 巫英伟, 黄洪涛, 张坤, 何梁, 叶天舟, 陈平

Effect of Surface Oxidation on Deuterium Permeation Performance of a Ferritic FeCrAl Alloy at 300-550 ℃
GAO Shixin, YIN Chunyu, WU Yingwei, HUANG Hongtao, ZHANG Kun, HE Liang, YE Tianzhou, CHEN Ping
表1 Fe-13Cr-4.5Al-2.2Mo-1.1Nb合金在不同温度点渗透数据
Table 1 Permeation test result of Fe-13Cr-4.5Al-2.2Mo-1.1Nb alloy at different temperatures
Temperature / ℃J / mol·m-2·s-1Ф / mol·m-1·s-1·MPa-1/2D / m2·s-1S / mol·m-3·MPa-1/2
3002.36×10-73.73 × 10-103.47 × 10-90.107
3607.37×10-71.16 × 10-94.60 × 10-90.253
4001.17×10-61.85 × 10-95.90 × 10-90.314
4501.99×10-63.16 × 10-98.03 × 10-90.394
5501.19 × 10-61.87 × 10-96.41 × 10-90.292