表2 铁尾矿基地聚物正交试验配合比
|
Table 2 Mix proportions of iron tailings-based geopolymers in orthogonal tests (kg/m3)
|
|
| Sample | Water glass | NaOH | Water | IT sand | Ceramic powder | IT powder |
|---|
| A | 231.64 | 57.83 | 173.46 | 1291.37 | 193.71 | 451.98 | | B | 323.61 | 61.39 | 135.82 | 1252.78 | 187.91 | 438.47 | | C | 426.94 | 62.71 | 88.95 | 1214.26 | 182.14 | 424.99 | | D | 380.43 | 55.88 | 70.24 | 1262.31 | 252.46 | 378.69 | | E | 312.79 | 78.09 | 140.81 | 1245.54 | 249.12 | 373.66 | | F | 269.46 | 51.12 | 201.76 | 1251.77 | 250.35 | 375.53 | | G | 377.85 | 71.68 | 69.77 | 1253.79 | 313.44 | 313.44 | | H | 317.06 | 46.57 | 142.70 | 1262.44 | 315.61 | 315.61 | | I | 267.65 | 66.82 | 200.42 | 1243.41 | 310.85 | 310.85 |
|
|
|