3.5%NaCl溶液中硝基巴比妥酸对AZ31BAZ91D镁合金腐蚀的缓蚀作用及机理研究
翟亚如, 熊金平, 赵景茂

Corrosion Inhibition Performance of Nitrobarbituric Acid on Mg-alloys AZ31B and AZ91D in 3.5%NaCl Solution
ZHAI Yaru, XIONG Jinping, ZHAO Jingmao
表3 AZ31B和AZ91D在25 ℃的含有1 g/L NBA的3.5%NaCl溶液中的析氢测试结果
Table 3 Hydrogen evolution results of AZ31B and AZ91D soaked in 3.5%NaCl solution with and without 1 g/L NBA
Mg-alloySolutionTime / hPH / mm·a-1ηHev / %
AZ31B3.5%NaCl240.1705-
480.1474-
720.1950-
3.5%NaCl + 1 g/L NBA240.16254.7
480.115621.6
720.094551.5
AZ91D3.5%NaCl240.0050-
480.0041-
720.0033-
3.5%NaCl + 1 g/L NBA240.0194-288.0
480.0122-197.6
720.0094-184.8