高速列车用铝合金环氧底漆的腐蚀行为和湿热老化机理研究
李丽, 李善文, 史洪微, 梁国平, 李春霖, 孙禹, 秦晋, 王伟, 韩恩厚

Corrosion Behavior and Hydrothermal Aging Mechanism of Epoxy Primer on Al-alloy for High-speed Train
LI Li, LI Shanwen, SHI Hongwei, LIANG Guoping, LI Chunlin, SUN Yu, QIN Jin, WANG Wei, HAN En-Hou
表1 环氧底漆/铝合金体系在3.5%NaCl溶液中浸泡不同时间后的EIS拟合结果
Table 1 Fitting results of EIS of epoxy primer coated Al-alloy immersed in 3.5%NaCl solution for different time
Immersion time / hRc / Ω·cm2QcWc / S·s1/2·cm-2
Y0 / S·sa·cm2a0
0.56.63 × 1086.10 × 10-108.64 × 10-1-
241.45 × 1095.99 × 10-108.65 × 10-1-
481.05 × 10103.97 × 10-108.93 × 10-1-
1201.25 × 10104.37 × 10-108.90 × 10-1-
3841.12 × 10104.50 × 10-108.92 × 10-1-
7201.09 × 10104.49 × 10-108.93 × 10-1-
12001.70 × 10104.14 × 10-109.00 × 10-1-
16801.32 × 10104.20 × 10-108.99 × 10-1-
21601.65 × 10104.19 × 10-109.00 × 10-1-
28802.23 × 1094.12 × 10-109.04 × 10-1-
38401.81 × 1095.11 × 10-108.87 × 10-1-
42009.79 × 1084.63 × 10-108.98 × 10-14.52 × 10-9