B10铜合金超双疏表面的制备及其性能研究
|
张吉昊, 徐亚程, 贾学远, 高荣杰
|
Preparation and Corrosion Resistance of Superamphiphobic Surface on B10 Cu-alloy
|
ZHANG Jihao, XU Yacheng, JIA Xueyuan, GAO Rongjie
|
|
表3 电化学拟合参数
|
Table 3 Electrochemical fitting parameters
|
|
Sample | Rs Ω·cm2 | CPE | Rf Ω·cm2 | Rct Ω·cm2 | Cdl F·cm-2 | η |
---|
Y0 / S⋅sec n | n |
---|
Bare | 2.451 | 5.301 × 10-4 | 0.7354 | 4.981 | 1224 | 3.228 × 10-7 | - | SA(0 d) | 4.418 | 8.042 × 10-5 | 0.6971 | 5.674 | 13560 | 4.326 × 10-7 | 90.97% | SA(1 d) | 4.774 | 6.891 × 10-4 | 0.6562 | 4.304 | 7598 | 7.242 × 10-7 | 83.89% | SA(3 d) | 3.151 | 3.752 × 10-4 | 0.6260 | 7.541 | 6196 | 4.122 × 10-7 | 80.25% | SA(5 d) | 5.201 | 3.662 × 10-4 | 0.6032 | 3.755 | 3587 | 3.919 × 10-7 | 65.88% |
|
|
|