温度对5Cr钢在模拟油田高温高压环境中CO2 腐蚀行为的影响
赵国仙, 刘冉冉, 丁浪勇, 张思琦, 郭梦龙, 王映超

Effect of Temperature on CO2-inducedCorrosion Behavior of 5Cr Steel in a Simulated Oilfield Produced High-temperature and High-pressured Water
ZHAO Guoxian, LIU Ranran, DING Langyong, ZHANG Siqi, GUO Menglong, WANG Yingchao
表2 5Cr钢在不同温度下腐蚀坑形貌的EDS分析结果 (mass fraction / %)
Table 2 EDS analysis results of the marked areas in Fig.5
Temperature / oCScan areaCOSClCaCrFe
50145.8338.85//0.260.732.40
218.6312.140.430.220.916.2660.52

70

114.4537.310.460.667.1130.547.48
220.2446.180.181.205.2421.325.15
326.1339.710.221.083.9515.5213.19
90111.2237.641.746.431.3014.3726.82
25.5934.781.566.601.6019.0130.53