温度对B10铜镍合金管冲刷腐蚀行为影响规律研究
王晓, 李明, 刘峰, 王忠平, 李相波, 李宁旺

Effect of Temperature on Erosion-corrosion Behavior of B10 Cu-Ni Alloy Pipe
WANG Xiao, LI Ming, LIU Feng, WANG Zhongping, LI Xiangbo, LI Ningwang
表3 B10管在不同温度海水中冲刷腐蚀不同时间的EIS拟合数据
Table 3 Fitting data of EIS of B10 pipe after erosion-corrosion at different temperatures for different time
Temperature / ℃Time / dRs / Ω·cm2CPE1 / μF·cm-2·S-nn1Rf / Ω·cm²CPE2 / μF·cm-2·S-nn2Rct / Ω·cm²
10028.044.090.85042,367342.10.696325.00
126.163.920.87423,110255.80.732427.31
329.722.460.75274,174462.40.657733.2
734.253.490.76544,779216.10.746738.32
1529.72.580.75293,722321.30.702540.48
3030.172.080.76224,882273.40.799142.61
25014.024.810.6875990283.90.794316.18
114.077.190.89831,554275.90.766619.49
318.019.380.75661,842215.70.809223.92
712.385.210.81131,943232.10.798624.34
1517.092.870.35742,040165.80.851926.72
309.842.040.79512,41058.390.937828.85
35014.907.090.7463390.4413.60.819710.10
112.877.750.7649870.4453.40.887515.17
312.389.490.70491,339301.90.880420.38
729.325.150.76541,492116.20.689221.89
157.657.840.7361637.2553.30.780714.68
3014.896.470.9495666.9577.40.703815.03
50018.998.820.9323323.4330.70.80099.27
124.666.530.9988343.6279.00.825213.72
316.065.220.7846367.3317.80.845217.03
718.696.750.7341381.8281.80.898918.45
1521.467.780.7246389.2271.30.825718.58
3026.226.640.8943348.2256.90.736113.23