Cl-与HSO3-对建筑用439不锈钢腐蚀行为的影响
|
陈昊, 樊志彬, 陈志坚, 周学杰, 郑鹏华, 吴军
|
Effect of Cl- and HSO3- on Corrosion Behavior of 439 Stainless Steel Used in Construction
|
CHEN Hao, FAN Zhibin, CHEN Zhijian, ZHOU Xuejie, ZHENG Penghua, WU Jun
|
|
表1 439不锈钢极化曲线及阻抗谱拟合参数
|
Table 1 Fitting electrochemical parameters of polarization curves and EIS of 439 stainless steel
|
|
NaCl (aq) | EcorrV | IcorrμA·cm-2 | Pitting potential / V | Passive areas V | RsΩ·cm-2 | Q1F·cm-2 | n1 | R1Ω·cm-2 | Q2F·cm-2 | n2 | R2Ω·cm-2 |
---|
3.5% | -0.071 | 0.119 | 0.320 | 0.231 | 46.94 | 1.20×10-5 | 0.87 | 4.96×104 | 1.93×10-5 | 0.65 | 4.05×105 | 6.0% | -0.099 | 0.164 | 0.286 | 0.264 | 27.85 | 1.22×10-5 | 0.91 | 1.38×104 | 2.09×10-5 | 0.64 | 3.67×105 | 10.0% | -0.218 | 0.518 | 0.092 | 0.190 | 18.94 | 4.00×10-5 | 0.83 | 1.21×104 | 5.73×10-5 | 0.40 | 1.24×105 | 14.0% | -0.175 | 0.509 | 0.183 | 0.238 | 17.13 | 4.71×10-5 | 0.91 | 8.14×103 | 2.74×10-5 | 0.66 | 2.13×105 | 18.0% | -0.140 | 0.285 | 0.160 | 0.180 | 12.29 | 1.62×10-5 | 0.92 | 8.59×103 | 2.52×10-5 | 0.61 | 2.71×105 |
|
|
|