尾矿库埋入式传感器不锈钢外壳腐蚀研究
|
王淇萱, 吕文生, 杨鹏, 诸利一, 廖文景, 朱远乐
|
Corrosion of Stainless Steel Shell of Embedded Sensor in Tailings Pond
|
WANG Qixuan, LYU Wensheng, YANG Peng, ZHU Liyi, LIAO Wenjing, ZHU Yuanle
|
|
表2 316L不锈钢试样在3种模拟液中浸泡不同时间的极化曲线的拟合结果
|
Table 2 Fitting electrochemical parameters of polarization curves of 316L stainless steel after immersion for different time in three simulated solutions
|
|
pH | Soaking time / d | EbVSCE | EcorrVSCE | IcorrμA∙cm-2 | pH | Soaking time / d | EbVSCE | EcorrVSCE | IcorrμA∙cm-2 | pH | Soaking time / d | EbVSCE | EcorrVSCE | IcorrμA∙cm-2 |
---|
| 0 | 0.763 | -0.147 | 1.410 | | 0 | 0.256 | -0.326 | 1.933 | | 0 | 0.224 | -0.167 | 0.096 | | 7 | 0.795 | 0.016 | 0.116 | | 7 | 0.390 | 0.034 | 0.027 | | 7 | 0.541 | -0.045 | 0.106 | | 15 | 0.801 | 0.034 | 0.148 | | 15 | 0.512 | -0.121 | 0.018 | | 15 | 0.353 | -0.086 | 0.127 | 1.5 | 30 | 0.840 | 0.160 | 0.120 | 3 | 30 | 0.525 | -0.116 | 0.153 | 7.5 | 30 | 0.477 | -0.133 | 0.038 | | 60 | 0.836 | 0.023 | 0.191 | | 60 | 0.420 | 0.027 | 0.082 | | 60 | 0.550 | -0.080 | 0.071 | | 120 | 0.810 | 0.111 | 0.103 | | 120 | 0.397 | -0.165 | 0.170 | | 120 | 0.456 | -0.176 | 0.171 | | 360 | 0.812 | 0.013 | 0.261 | | 360 | 0.480 | -0.294 | 0.875 | | 360 | 0.530 | -0.239 | 0.698 |
|
|
|