表2 通过拟合Q235钢在含有不同缓蚀剂的CO2/H2S共存盐水溶液中测得的极化曲线得到的电化学参数
Table 2 Electrochemical parameters fitted from the polarization curves of Q235 steel in CO2/H2S coexistent brine solutions containing different inhibitors
Inhibitonβa / mV·dec-1βc / mV·dec-1Ecorrvs SCE / mVIcorr / μA·cm-2ηp / %
Blank56.6-198.4-746.5168.4---
5 mg/L IAS+5 mg/L DTAB58.1-181.7-679.18.295.1
5 mg/L IAS+5 mg/L TTAB54.8-223.6-705.925.285.0
5 mg/L IAS+5 mg/L CTAB55.9-207.9-738.879.952.6