固溶处理制度对挤压态Mg-Zn-Y-Nd镁合金在模拟体液中腐蚀和析氢行为的影响规律研究
郏义征, 王保杰, 赵明君, 许道奎

Effect of Solid Solution Treatment on Corrosion and Hydrogen Evolution Behavior of an As-extruded Mg-Zn-Y-Nd Alloy in an Artificial Body Fluid
JIA Yizheng, WANG Baojie, ZHAO Mingjun, XU Daokui
表1 固溶处理前后挤压态Mg-6Zn-1.2Y-0.8Nd合金样品极化曲线的拟合结果
Table 1 Fitted parameters of polarization curves of as-extruded Mg-6Zn-1.2Y-0.8Nd alloy before and after T4 treatment
ConditionPre-immersion time / hEcorrVSCEIcorr10-3 mA·cm-2
Before T40-1.574±0.157.9±0.5
After T40-1.572±0.154.8±0.2
Before T42-1.581±0.205.0±0.3
After T42-1.624±0.153.6±0.2
Before T44-1.525±0.104.1±0.3
After T44-1.625±0.153.1±0.3
Before T48-1.612±0.103.4±0.3
After T48-1.606±0.152.0±0.1
Before T424-1.620±0.252.2±0.2
After T424-1.568±0.151.2±0.1
Before T448-1.633±0.102.9±0.1
After T448-1.584±0.151.9±0.1