Corten-A耐候钢在模拟污染海洋大气环境中的加速腐蚀相关性研究
冯亚丽,白子恒,陈利红,魏丹,张东玖,姚琼,吴俊升,董超芳,肖葵

Correlation of Indoor Accelerated Corrosion with Outdoor Exposure for Corten-A Weathering Steel in Polluted Marine Atmospheric Environments
Yali FENG,Ziheng BAI,Lihong CHEN,Dan WEI,Dongjiu ZHANG,Qiong YAO,Junsheng WU,Chaofang DONG,Kui XIAO
表6 青岛地区腐蚀失重的绝对差
Table 6 Absolute difference of corrosion mass loss in Qingdao
Test time1%NaCl2%NaCl3.5%NaCl5%NaCl7%NaCl
Δ01Δ02Δ03Δ04Δ05
1 a (216 h)00000
2 a (432 h)0.12010.28580.32760.38850.2634
4 a (864 h)0.38500.96341.11771.34910.8819
8 a (1728 h)0.92562.44102.86893.52862.2188
12 a (2592 h)1.45793.96794.70055.84813.5914
16 a (3456 h)1.97915.51046.56528.23684.9721