Corten-A耐候钢在模拟污染海洋大气环境中的加速腐蚀相关性研究
冯亚丽,白子恒,陈利红,魏丹,张东玖,姚琼,吴俊升,董超芳,肖葵

Correlation of Indoor Accelerated Corrosion with Outdoor Exposure for Corten-A Weathering Steel in Polluted Marine Atmospheric Environments
Yali FENG,Ziheng BAI,Lihong CHEN,Dan WEI,Dongjiu ZHANG,Qiong YAO,Junsheng WU,Chaofang DONG,Kui XIAO
表5 万宁地区腐蚀失重数据预处理结果
Table 5 Pretreatment results of corrosion mass loss in Wanning
Test timeOutdoor exposure1%NaCl2%NaCl3.5%NaCl5%NaCl7%NaCl
Y0Y1Y2Y3Y4Y5
1 a (72 h)1.00001.00001.00001.00001.00001.0000
2 a (144 h)1.18311.66221.8281.86971.93061.8055
4 a (288 h)1.39962.76303.34153.49583.72723.2600
8 a (576 h)1.65574.59296.10826.53617.19585.8860
12 a (864 h)1.82697.28168.69289.425310.57308.3162
16 a (1152 h)1.959012.103811.165712.220613.892210.6274