Corten-A耐候钢在模拟污染海洋大气环境中的加速腐蚀相关性研究
冯亚丽,白子恒,陈利红,魏丹,张东玖,姚琼,吴俊升,董超芳,肖葵

Correlation of Indoor Accelerated Corrosion with Outdoor Exposure for Corten-A Weathering Steel in Polluted Marine Atmospheric Environments
Yali FENG,Ziheng BAI,Lihong CHEN,Dan WEI,Dongjiu ZHANG,Qiong YAO,Junsheng WU,Chaofang DONG,Kui XIAO
表3 万宁地区腐蚀失重量统计 (mass loss / (g·m-2))
Table 3 Statistic of corrosion mass loss in Wanning (mass loss / (g·m-2))
Test timeOutdoor exposure1%NaCl2%NaCl3.5%NaCl5%NaCl7%NaCl
X0X1X2X3X4X5
1 a (72 h)385.83210.50180.73142.09120.66142.25
2 a (144 h)456.48349.90330.37265.66232.94256.83
4 a (288 h)540.00581.63603.90496.71449.72463.73
8 a (576 h)638.83966.801103.92928.69868.23837.27
12 a (864 h)704.851301.481571.011339.211275.721182.97
16 a (1152 h)755.801607.062017.941736.381676.211511.73