Corten-A耐候钢在模拟污染海洋大气环境中的加速腐蚀相关性研究
冯亚丽,白子恒,陈利红,魏丹,张东玖,姚琼,吴俊升,董超芳,肖葵

Correlation of Indoor Accelerated Corrosion with Outdoor Exposure for Corten-A Weathering Steel in Polluted Marine Atmospheric Environments
Yali FENG,Ziheng BAI,Lihong CHEN,Dan WEI,Dongjiu ZHANG,Qiong YAO,Junsheng WU,Chaofang DONG,Kui XIAO
表2 青岛地区腐蚀失重量统计 (mass loss / (g·m-2))
Table 2 Statistic of corrosion mass loss in Qingdao (mass loss / (g·m-2))
Test timeOutdoor exposure1%NaCl2%NaCl3.5%NaCl5%NaCl7%NaCl
X0X1X2X3X4X5
1 a (216 h)535.45471.03470.15383.09342.27362.88
2 a (432 h)825.74782.96859.43716.27660.79655.19
4 a (864 h)1273.351301.481571.011339.211275.721182.97
8 a (1728 h)1963.602163.372871.782503.932462.912135.90
12 a (2592 h)2529.902912.244086.913610.763618.833017.77
16 a (3456 h)3028.143596.045249.564681.614754.903856.45