Corrosion Behavior of Extruded EW75 Mg-alloy in Shenyang Industrial Atmosphere
SUN Shuo1, DAI Jiaming1, SONG Yingwei2(), AI Caijiao3
1.School of Environmental and Chemical Engineering, Shenyang University of Technology, Shenyang 110870, China
2.Key Laboratory of Nuclear Materials and Safety Assessment, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
3.Shandong Key Laboratory Advanced Aluminum Materials and Technology, Binzhou Institute of Technology, Binzhou 256600, China
Cite this article: 

SUN Shuo, DAI Jiaming, SONG Yingwei, AI Caijiao. Corrosion Behavior of Extruded EW75 Mg-alloy in Shenyang Industrial Atmosphere. Journal of Chinese Society for Corrosion and protection, 2024, 44(1): 141-150.

Download:  HTML  PDF(16882KB) 
Export:  BibTeX | EndNote (RIS)      
Abstract  

Mg-alloys as the lightest metallic structural materials have many excellent properties, but their corrosion resistance is poor. Thus the corrosion behavior of Mg-alloy in different service conditions need to be acquired. Especially, the composition of pollutants and meteorological factors in different atmospheric environments may affect the corrosion behavior of Mg-alloys. In this paper, the corrosion behavior of the extruded EW75 Mg-alloy in Shenyang industrial atmosphere was investigated by atmospheric exposure at Shenyang atmospheric test station located at 123°26' east and 41°46' north. After exposure for different durations, the test alloys were characterized by means of SEM, EDS and Raman spectroscopy in terms of their surface and cross sectional morphology and the chemical composition of corrosion products. The results show that the dusts containing soluble salts in the industrial atmosphere were deposited on the surface of the extruded EW75 Mg-alloy and form round-shaped corrosion products, which show good protection for the corresponding magnesium matrix; the potential difference between the fine precipitation phases and α-Mg is low, which exhibits weak micro-galvanic effect, resulting in the formation of uniform corrosion. In addition, the corrosion rate of Mg-alloys in Shenyang atmosphere is greatly influenced by seasonal variations. Compared with the low temperature and low humidity winter, the corrosion rate of the extruded EW75 Mg-alloy is significantly higher in the high temperature and high humidity summer.

Key words:  rare-earth Mg-alloy      atmospheric corrosion      corrosion resistance      industrial atmosphere      micro-galvanic corrosion     
Received:  16 March 2023      32134.14.1005.4537.2023.070
ZTFLH:  TG174  
Fund: National Natural Science Foundation of China(52171086);National R&D Infrastructure and Facility Development Program of China(2005DKA10400-15-Z04);the Bintech‐IMR R&D Program(GYY-JSBU-2022-005)
Corresponding Authors:  SONG Yingwei, E-mail: ywsong@imr.ac.cn

URL: 

https://www.jcscp.org/EN/10.11902/1005.4537.2023.070     OR     https://www.jcscp.org/EN/Y2024/V44/I1/141

Date

Rainfall

mm

Rainfall time

d

Temperature / oCRH / %
Monthly maximum

Monthly

minimum

Monthly

average

Monthly maximum

Monthly

minimum

Monthly

average

2021.0784.49341926.5984277.8
2021.0888.512301322.5983174.8
2021.09199.31527617.4992674.6
2021.1037.8322-59992065.2
2021.1148.8812-12-1.9982167.3
2021.123.439-19-6.1972054.8
2022.010.323-22-11842451.3
2022.027.5410-21-5931952
2022.0330718-84.597953.9
2022.0410429213.4931145.9
2022.0586.4933418.51001456
2022.06319.820311122.41004681.9
Table 1  Meteorological data of Shenyang city during the whole exposure test
Fig.1  Low (a) and high (b) magnified surface morphologies of extruded EW75 Mg-alloy
Fig.2  Optical corrosion images of the extruded EW75 Mg-alloy exposed to Shenyang atmosphere for different durations: (a) 1 month, (b) 3 months, (c) 6 months, (d) 12 months
Fig.3  Surface corrosion morphologies of the extruded EW75 Mg-alloy exposed to Shenyang atmosphere for different durations: (a) 1 month, (b) 3 months, (c) 6 months, (d) 12 months
ElementsMgOSiSCa
Rod-like product12.1432.9554.91--
Round product47.8044.342.802.302.76
Table 2  EDS analysis results of the corrosion products in Fig.3a (mass fraction / %)
Fig.4  Raman spectrum of the corrosion products formed on the extruded EW75 Mg-alloy exposed to Shenyang atmosphere for 1 a
PositionMgCOAlYSiSClCaFeGd
A30.8215.7840.941.580.824.231.480.393.96--
B34.6515.7645.100.90-1.200.28-1.370.74-
C56.11-41.09--1.47-1.33---
D43.416.9028.40-6.21-1.12-1.71-12.24
Table 3  EDS analysis results of the corrosion products in Fig.5 (mass fraction / %)
Fig.5  Morphologies of the round corrosion products formed on the extruded EW75 Mg-alloy exposed to Shenyang atmosphere for 12 months (a, b), cross-sectional morphology of the round corrosion product (c), and enlarged view of the area marked by white circle in Fig.5b (d)
Fig.6  Surface corrosion morphologies of the extruded EW75 Mg-alloy after exposure in Shenyang atmosphere for different durations and then removing corrosion products: (a, b) 1 month, (c, d) 3 months, (e, f) 6 months, (g, h) 12 months
Fig.7  Cross-sectional corrosion morphologies of the extruded EW75 Mg-alloy after exposure in Shenyang atmosphere for different durations and then removing corrosion products: (a) 1 month, (b) 3 months, (c) 6 months, (d) 12 months
Fig.8  Variation of corrosion rate of the extruded EW75 Mg-alloy with exposure time
Fig.9  Cross-sectional morphology of the corrosion products formed on the extruded EW75 Mg-alloy exposed to Shenyang atmosphere for 11 months
Fig.10  Schematic diagrams of corrosion mechanism of the extruded EW75 Mg-alloy in the initial stage of exposure in industrial atmosphere: (a) electrochemical corrosion under thin electrolyte film, (b) corrosion after evaporation of thin electrolyte film
1 Li X, Zhang C, Wang J S, et al. Research progress on corrosion behavior and protection technology of magnesium alloys [J]. Aeronaut. Manuf. Technol., 2021, 64(19): 59
李 鑫, 张 弛, 王俊升 等. 镁合金腐蚀行为与防护技术研究进展 [J]. 航空制造技术, 2021, 64(19): 59
2 Tang Z F, Liu X K, Ren G M. Requirements for the use of magnesium alloy materials in aircraft engine airworthiness standards [J]. Aeronaut. Stand. Qual., 2014, (6): 26
唐正府, 刘兴科, 任光明. 航空发动机适航标准中镁合金材料使用要求 [J]. 航空标准化与质量, 2014, (6): 26
3 Li S Y, Zheng D R. Development and analysis of magnesium alloy components of new energy vehicles [J]. J. New Ind., 2019, 9(1): 66
李淑英, 郑德润. 新能源汽车镁合金零部件的开发分析 [J]. 新型工业化, 2019, 9(1): 66
4 Song G L, Atrens A. Corrosion mechanisms of magnesium alloys [J]. Adv. Eng. Mater., 1999, 1: 11
doi: 10.1002/(ISSN)1527-2648
5 Zeng X Q. Research and application progress of rare earth magnesium alloy [J]. Rare Earth Inf., 2016, (2): 26
曾小勤. 稀土镁合金研究与应用进展 [J]. 稀土信息, 2016, (2): 26
6 Zhang X, Zhang K, Li X G, et al. Comparative study on corrosion behavior of as-cast and extruded Mg-5Y-7Gd-1Nd-0.5Zr alloy in 5% NaCl aqueous solution [J]. Trans. Nonferrous Met. Soc. China, 2012, 22: 1018
doi: 10.1016/S1003-6326(11)61278-8
7 Liu J H, Song Y W, Chen J C, et al. The special role of anodic second phases in the micro-galvanic corrosion of EW75 Mg alloy [J]. Electrochim. Acta, 2016, 189: 190
doi: 10.1016/j.electacta.2015.12.075
8 Feng B J, Liu G N, Yang P X, et al. Different role of second phase in the micro-galvanic corrosion of WE43 Mg alloy in NaCl and Na2SO4 solution [J]. J. Magnes. Alloy., 2022, 10: 1598
doi: 10.1016/j.jma.2020.12.013
9 Wang F P, Li X G, Lin C, et al. Atmospheric corrosion behavior of AZ91D magnesium alloy in Beijing area [J]. J. Chin. Soc. Corros. Prot., 2004, 24: 345
王凤平, 李晓刚, 林 翠 等. AZ91D镁合金在北京地区的大气腐蚀行为研究 [J]. 中国腐蚀与防护学报, 2004, 24: 345
10 Lin C, Li X G, Li M, et al. Corrosion behavior of AZ91D magnesium alloy in city atmosphere [J]. Acta Metall. Sin., 2004, 40: 191
林 翠, 李晓刚, 李 明 等. Mg合金AZ91D在城市大气环境中的腐蚀行为 [J]. 金属学报, 2004, 40: 191
11 Xia L T, Li J Y, Wang R F. Industrial atmospheric corrosion behavior of AZ91D magnesium alloy in Linfen city [J]. China Foundry Mach. Technol., 2009, 44(3): 15
夏兰廷, 李晋英, 王荣峰. AZ91D镁合金在临汾工业大气中的腐蚀行为 [J]. 中国铸造装备与技术, 2009, 44(3): 15
12 Gong P, Cao X J, Ning S Q, et al. Influence of different environments on atmospheric corrosion of AZ61 magnesium alloy [J]. China Surf. Eng., 2015, 28: 123
龚 沛, 曹学军, 宁韶奇 等. 不同环境对AZ61镁合金大气腐蚀的影响 [J]. 中国表面工程, 2015, 28: 123
13 Jiang Q T, Zhang K, Li X G, et al. Atmospheric corrosion of Mg-rare earth alloy in typical inland and marine environments [J]. Corros. Eng. Sci. Technol., 2014, 49: 651
doi: 10.1179/1743278214Y.0000000163
14 Song Y W, Liu D, Tang W N, et al. Comparison of the corrosion behavior of AM60 Mg alloy with and without self-healing coating in atmospheric environment [J]. J. Magnes. Alloy., 2021, 9: 1220
doi: 10.1016/j.jma.2020.05.018
15 Jiang Q T. The research of EW75 magnesium alloy on the atmospheric corrosion behaviors [D]. Beijing: General Research Institute for Nonferrous Metals, 2014
蒋全通. EW75镁合金大气腐蚀行为研究 [D]. 北京: 北京有色金属研究总院, 2014
16 Wang Y Y. Typical corrosion appearance of metals [J]. Equip. Environ. Eng., 2006, 3(4): 31
王曰义. 金属的典型腐蚀形貌 [J]. 装备环境工程, 2006, 3(4): 31
17 Wang Z G, Hai C, Jiang J, et al. Corrosion behavior of Q235 steels in atmosphere at Deyang district for one Year [J]. J. Chin. Soc. Corros. Prot., 2021, 41: 871
王志高, 海 潮, 姜 杰 等. Q235钢在德阳大气环境中腐蚀行为研究 [J]. 中国腐蚀与防护学报, 2021, 41: 871
doi: 10.11902/1005.4537.2020.180
18 Cui Z Y, Ge F, Wang X. Corrosion mechanism of materials in three typical harsh marine atmospheric environments [J]. J. Chin. Soc. Corros. Prot., 2022, 42: 403
崔中雨, 葛 峰, 王 昕. 几种苛刻海洋大气环境下的海工材料腐蚀机制 [J]. 中国腐蚀与防护学报, 2022, 42: 403
doi: 10.11902/1005.4537.2021.165
19 Guo R, Lin X Y. Corrosive characteristics of dust particles [J]. Electromech. Compon., 2004, 24(1): 3
郭 锐, 林雪燕. 尘土颗粒的腐蚀特性 [J]. 机电元件, 2004, 24(1): 3
20 Liu Y C, He H. Analysis of chemical composition of atmospheric particles [J]. Prog. Chem., 2007, 19: 1620
刘永春, 贺 泓. 大气颗粒物化学组成分析 [J]. 化学进展, 2007, 19: 1620
21 Zhang D D, Zhao C Y, Wang C, et al. Atmospheric aerosols corrosion [J]. J. Chin. Soc. Corros. Prot., 2015, 35: 91
张丹丹, 赵春英, 汪 川 等. 大气气溶胶腐蚀 [J]. 中国腐蚀与防护学报, 2015, 35: 91
doi: 10.11902/1005.4537.2014.083
22 Liu J H, Song Y W, Shan D Y, et al. Comparative study on corrosion behavior of cast and forged Mg-5Y-7Gd-1Nd-0.5Zr alloys [J]. Acta Metall. Sin., 2018, 54: 1141
doi: 10.11900/0412.1961.2017.00484
刘金辉, 宋影伟, 单大勇 等. 铸态和锻造态Mg-5Y-7Gd-1Nd-0.5Zr合金腐蚀行为对比研究 [J]. 金属学报, 2018, 54: 1141
doi: 10.11900/0412.1961.2017.00484
23 Li L, Li X G, Dong C F, et al. Research method development of corrosion under droplets during atmospheric corrosion [J]. Corros. Prot., 2010, 31: 260
李 磊, 李晓刚, 董超芳 等. 大气腐蚀中液滴覆盖下腐蚀现象的研究方法进展 [J]. 腐蚀与防护, 2010, 31: 260
24 Liang L H, Wang J, Jiang J. Effects of micro-droplets on atmospheric corrosion process [J]. Corros. Sci. Prot. Technol., 2010, 22: 504
梁利花, 王 佳, 姜 晶. 微液滴在大气腐蚀过程中的作用 [J]. 腐蚀科学与防护技术, 2010, 22: 504
25 Zhao D, Bian S S, Wang S, et al. Component characteristics and source apportionment of ambient air PM2.5 at multi-seasons in Shenyang [J]. Environ. Prot. Sci., 2021, 47: 128
赵 帝, 卞思思, 王 帅 等. 沈阳市分季节环境空气PM2.5组分特征分析与来源解析 [J]. 环境保护科学, 2021, 47: 128
26 Wang G Z, Ren W H, Yu X N, et al. Characteristics and sources of water-soluble ion pollution in PM2.5 in winter in Shenyang [J]. Environ. Sci., 2021, 42: 30
王国祯, 任万辉, 于兴娜 等. 沈阳市冬季大气PM2.5中水溶性离子污染特征及来源解析 [J]. 环境科学, 2021, 42: 30
27 Bian S S, Zhao D, Wang W K, et al. Variation characteristics and source analysis of water-soluble ions in PM2.5 during winter in Shenyang [J]. Environ. Prot. Sci., 2021, 47(3): 129
卞思思, 赵 帝, 王维宽 等. 沈阳冬季PM2.5中水溶性离子变化特征及来源分析 [J]. 环境保护科学, 2021, 47(3): 129
[1] LIU Guoqiang, ZHANG Dongfang, CHEN Haoxiang, FAN Zhihong, XIONG Jianbo, WU Qingfa. Electrochemical Corrosion Behavior of 2304 Duplex Stainless Steel in a Simulated Pore Solution in Reinforced Concrete Serving in Marine Environment[J]. 中国腐蚀与防护学报, 2024, 44(1): 204-212.
[2] XIE Yun, LIU Ting, WANG Wen, ZHOU Jialin, TANG Song. Effect of Microstructure on Corrosion Resistance of a High-strength Ultralightweight Mg-Li Alloy[J]. 中国腐蚀与防护学报, 2024, 44(1): 255-260.
[3] WANG Jingyu, ZHOU Xuejie, WANG Honglun, WU Jun, CHEN Hao, ZHENG Penghua. Initial Corrosion Behavior of Carbon Steel and High Strength Steel in South China Sea Atmosphere[J]. 中国腐蚀与防护学报, 2024, 44(1): 237-245.
[4] SHANG Ting, JIANG Guangrui, LIU Guanghui, QIN Hancheng. Effect of Heat Treatment Process on Microstructure and Corrosion Resistance of Zn-6%Al-3%Mg Coating[J]. 中国腐蚀与防护学报, 2023, 43(6): 1413-1418.
[5] XIAO Wentao, LIU Jing, PENG Jingjing, ZHANG Xian, WU Kaiming. Corrosion Resistance of Two Arc Spraying Coatings on EH36 Steel in Neutral Salt Spray Environment[J]. 中国腐蚀与防护学报, 2023, 43(5): 1003-1014.
[6] YANG Haifeng, YUAN Zhizhong, LI Jian, ZHOU Naipeng, GAO Feng. Effect of Ni Content on Corrosion Behavior of Cu-bearing Aged Weldable Steels in a Simulated Tropical Marine Atmosphere[J]. 中国腐蚀与防护学报, 2023, 43(5): 1022-1030.
[7] CHEN Xiaohan, BAI Yang, WANG Zhichao, CHEN Congzong, ZHANG Yong, CUI Xianlin, ZUO Juanjuan, WANG Tongliang. Preparation and Corrosion Resistance of Surface Tolerant Epoxy Anti-corrosion Primer[J]. 中国腐蚀与防护学报, 2023, 43(5): 1126-1132.
[8] WANG Yang, LIU Yuanhai, MU Xianlian, LIU Miaoran, WANG Jun, LI Qiuping, CHEN Chuan. Effect of Environmental Factors on Material Transfer in Thin Liquid Film During Atmospheric Corrosion Process in Marine Environment[J]. 中国腐蚀与防护学报, 2023, 43(5): 1015-1021.
[9] DING Li, ZOU Wenjie, ZHANG Xuejiao, CHEN Jun. Silicon-Zirconium Composite Conversion Film on ADC12 Aluminum Alloy[J]. 中国腐蚀与防护学报, 2023, 43(4): 903-910.
[10] LIU Chao, CHEN Tianqi, LI Xiaogang. Research Progress on Initiation Mechanism of Local Corrosion Induced by Inclusions in Low Alloy Steel[J]. 中国腐蚀与防护学报, 2023, 43(4): 746-754.
[11] ZOU Wenjie, DING Li, ZHANG Xuejiao, CHEN Jun. Epoxy/Organosiloxane Modified Cationic Acrylic Emulsion Composite Coating[J]. 中国腐蚀与防护学报, 2023, 43(4): 922-928.
[12] XIAO Meng, WANG Qinying, ZHANG Xingshou, XI Yuchen, BAI Shulin, DONG Lijin, ZHANG Jin, YANG Junjie. Effect of Laser Quenching on Microstructure, Corrosion and Wear Behavior of AISI 4130 Steel[J]. 中国腐蚀与防护学报, 2023, 43(4): 713-724.
[13] WU Duoli, WU Haotian, SUN Hui, SHI Jianjun, WEI Xinlong, ZHANG Chao. Research Status and Development of Laser Cladding High Temperature Protective Coating[J]. 中国腐蚀与防护学报, 2023, 43(4): 725-736.
[14] WU Jiahao, WU Liang, YAO Wenhui, YUAN Yuan, XIE Zhihui, WANG Jingfeng, PAN Fusheng. Properties of Layered Dihydroxyl Metal (MgAlLa) Oxide Composite Coatings on Different Micro-arc Oxidation Surfaces of Mg-Gd-Y-Zn-Mn Alloy[J]. 中国腐蚀与防护学报, 2023, 43(4): 693-703.
[15] NI Ya, SHI Fangchang, QI Jiqiu. Effect of Ce on Microstructure and Corrosion Resistance of Zn-0.6Cu-0.3Ti Alloy[J]. 中国腐蚀与防护学报, 2023, 43(4): 803-811.
No Suggested Reading articles found!